TECHNET Archives

October 2005

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
TechNet E-Mail Forum <[log in to unmask]>
Date:
Wed, 19 Oct 2005 13:53:14 -0500
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, Franklin Asbell <[log in to unmask]>
Subject:
From:
Franklin Asbell <[log in to unmask]>
Content-Transfer-Encoding:
7bit
In-Reply-To:
Content-Type:
text/plain; charset="US-ASCII"
MIME-Version:
1.0
Parts/Attachments:
text/plain (293 lines)
I would agree in some form of contaminate between layers from looking at
those latest pictures.

I would not conclude moisture or water as there is not enough information.

If I were examining those, certainly, I would look for some type of staining
in the center of the separated layers.

Franklin

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Brummer Chuck
Sent: Wednesday, October 19, 2005 1:46 PM
To: [log in to unmask]
Subject: Re: [TN] Delamination at Thermal Via area?

Hi,

I stayed quiet before because it looked like several people had some great
clues to your problem.
But with these other pictures, it would appear to me that there was a
problem with moisture or water in the lay up.  If you cut a blister an smell
ammonia, then there was water present when the board was laminated.

Chuck Brummer
Siemens/AIM


-----Original Message-----
From: Steve Gregory [mailto:[log in to unmask]]
Sent: Wednesday, October 19, 2005 10:49 AM
To: [log in to unmask]
Subject: Re: [TN] Delamination at Thermal Via area?


Hi George!

Got your pictures up! Check out:

http://www.stevezeva.homestead.com/files/Delamination_Blisters-1.jpg
http://www.stevezeva.homestead.com/files/Delamination_Blisters-2.jpg
http://www.stevezeva.homestead.com/files/Delamination_Blisters-3.jpg

Kind regards,

-Steve Gregory-
Senior Process Engineer
LaBarge Incorporated
Tulsa, Oklahoma
(918) 459-2285
(918) 459-2350 FAX



|---------+---------------------------->
|         |           "Wenger, George  |
|         |           M."              |
|         |           <George.Wenger@an|
|         |           drew.com>        |
|         |                            |
|         |           10/19/2005 11:00 |
|         |           AM               |
|         |                            |
|---------+---------------------------->

>---------------------------------------------------------------------------
-----------------------------------|
  |
|
  |       To:       TechNet E-Mail Forum <[log in to unmask]>@SMTP@Exchange,
Stephen R Gregory/LABARGE@LABARGE      |
  |       cc:
|
  |       Subject:  RE: [TN] Delamination at Thermal Via area?
|

>---------------------------------------------------------------------------
-----------------------------------|



Wee Mei,

I've asked Steve to post three images of delamination blistering that
might be different than you are seeing but the cause is most likely the
same.  I do not know how many layers there are or the number of thermal
vias there are in the heat spreader portion of the U2 footprint on your
board but it appears that your delamination is occurring in an area of
the board where the outside layers are totally covered by metal (i.e.,
copper).  This is decrease the ability of the board to outgas in those
areas if the board is heated too rapidly or to too high a temperature.
I'm also assuming but can't tell because I haven't seen a cross section
of your thermal vias but my guess would be that you do not have good
attachment integrity of the outer-layer copper to the barrels of the
thermal vias and therefore the thermal vias are not providing any
mechanical strength to hole you board together when reflowed.  The three
images I've sent to Steve show delamination blisters on the bottom side
of a 14-Layer PCB.  The delamination is occurring between layer 13 and
layer 14 in areas that have a copper ground plane on Layer 14.  There
acre also not PTH's in these areas to hold the board together when
internal moisture is driven off too fast.  There are no blisters where
ever there are PTH's.  We're not sure there was a single cause for our
delamination or multiple causes.  These boards were over 1 year old and
could have and probably did absorb moisture from the environment.  We
believe the reflow profile that caused these blisters had too fast a
ramp and too hot a peak temperature.  If we baked the boards prior to
the reflow they didn't delamination or if we didn't bake the boards and
used a correct profile they didn't blister.  I hope this information
helps you find the root cause for you delamination.  My suggestion is to
examine your reflow profile and cross section thermal vias in the
blistered area.


Regards,
George
George M. Wenger
Reliability / FMA Engineer
Base Station and Subsystems Group
Andrew Corporation, 40 Technology Drive, Warren, NJ 07059 (908) 546-4531
[log in to unmask]

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Steve Gregory
Sent: Wednesday, October 19, 2005 10:30 AM
To: [log in to unmask]
Subject: Re: [TN] Delamination at Thermal Via area?

Hi Wee Mei!

I've got your pictures posted. Go to:

http://www.stevezeva.homestead.com/files/U2_top.JPG
http://www.stevezeva.homestead.com/files/U2_bottom.JPG
http://www.stevezeva.homestead.com/files/U2_delamination.JPG

Are the vias filled? Are you seeing this delamination on very many
PCB's? Are you seeing it only on the bottom of the PCB?

Kind regards,

-Steve Gregory-
Senior Process Engineer
LaBarge Incorporated
Tulsa, Oklahoma
(918) 459-2285
(918) 459-2350 FAX



|---------+---------------------------->
|         |           Wee Mei          |
|         |           <[log in to unmask]
|         |           SG>              |
|         |           Sent by: TechNet |
|         |           <[log in to unmask]>|
|         |                            |
|         |                            |
|         |           10/19/2005 03:47 |
|         |           AM               |
|         |           Please respond to|
|         |           TechNet E-Mail   |
|         |           Forum            |
|         |           <[log in to unmask]>|
|         |           ; Please respond |
|         |           to Wee Mei       |
|         |           <[log in to unmask]
|         |           SG>              |
|         |                            |
|---------+---------------------------->

>-----------------------------------------------------------------------
---------------------------------------|
  |
|
  |       To:       [log in to unmask]@SMTP@Exchange
|
  |       cc:       (bcc: Stephen R Gregory/LABARGE)
|
  |       Subject:  [TN] Delamination at Thermal Via area?
|

>-----------------------------------------------------------------------
---------------------------------------|



Hello,

Just asked Steve to download 3 pictures on the defects. Kindly take a
look at them and would appreciate some feedback on the possible root
cause.

Steve : Thanks for the downloading.

Regards,
Wee Mei

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing
per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask]
or 847-615-7100 ext.2815
-----------------------------------------------------



__________________________________________________________________
This message may contain information that is privileged and confidential
to LaBarge, Inc.  It is for use only by the individual or entity named
above.
If you are not the intended recipient, you may not copy, use or deliver
this message to anyone.  In such event, you should destroy the message
and kindly notify the sender by reply e-mail.

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
archives of previous posts at: http://listserv.ipc.org/archives Please
visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------

----------------------------------------------------------------------------
--------------------
This message is for the designated recipient only and may
contain privileged, proprietary, or otherwise private information.
If you have received it in error, please notify the sender
immediately and delete the original.  Any unauthorized use of
this email is prohibited.
----------------------------------------------------------------------------
--------------------
[mf2]



__________________________________________________________________
This message may contain information that is privileged and confidential to
LaBarge, Inc.  It is for use only by the individual or entity named above.
If you are not the intended recipient, you may not copy, use or deliver
this message to anyone.  In such event, you should destroy the message and
kindly notify the sender by reply e-mail.

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2