I'm guessing no- or low- flow prepreg was "not" used, as these are the blind
vias, epoxy oozed out at lamination, the panel(s) was/were not planarized,
the epoxy was plated over (permanganate, then electroless, then electrolytic
copper processes) and the solder (HASL) coated over the existing copper
bump.
Franklin
-----Original Message-----
From: Brooks,Bill [mailto:[log in to unmask]]
Sent: Monday, September 12, 2005 2:54 PM
To: [log in to unmask]
Subject: [TN] raised vias...
Can someone give us a read on what they think cause the raised vias on
Steve's website picture? http://www.stevezeva.homestead.com page 2.
Bill Brooks - KG6VVP
PCB Design Engineer, C.I.D.+, C.I.I.
Tel: (760)597-1500 Ext 3772 Fax: (760)597-1510
Datron World Communications, Inc.
_______________________________________
San Diego Chapter of the IPC Designers Council
Communications Officer, Web Manager
http://dcchapters.ipc.org/SanDiego/
http://pcbwizards.com
-----Original Message-----
From: Steve Gregory [mailto:[log in to unmask]]
Sent: Monday, September 12, 2005 2:28 PM
To: [log in to unmask]
Subject: Re: [DC] Raised vias
Hi Fred and Everybody!
Speaking of "Raised Vias" and "Anthills", I have some anthills on some
Boards that we're building here now.
The anthills aren't from plugging or anything, but are blind via in pad.
I thought that they wouldn't present too much of a problem because I
thought that after printing paste and reflow, everything would level
out...but that wasn't the case.
At locations where I was placing something called a PowerPAK SO8, there was
open solder defects at some of the joints because (I think) of the raised
vias. You can see the PowerPAK part drawing, and the raised vias that I'm
talking about on my web page at: http://www.stevezeva.homestead.com . Go to
"Picture Page 2" and look for "PowerPAK SO8 and Raised Vias".
I don't have a clue why the vias are raised like that...maybe that's a
question for the TechNet.
Kind regards,
-Steve Gregory-
Senior Process Engineer
LaBarge Incorporated
Tulsa, Oklahoma
(918) 459-2285
(918) 459-2350 FAX
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|