Hi Juan! I recommend you try George's suggestion - the old rule thumb comes
into play as "like dissolves like" - take a small amount of the 615 flux
and apply it to the white residue. If it has completely changed its
chemical character then the 615 may allow you to remove it. As Brian
suggested, you are going to need to mechanically scrub the residue to
promote its removal. Good Luck.
Dave Hillman
Rockwell Collins
[log in to unmask]
"Juan T. Marugán"
<[log in to unmask]
ES> To
Sent by: TechNet [log in to unmask]
<[log in to unmask]> cc
Subject
09/07/2005 06:22 Re: [TN] Cleaning rosin flux
AM residues
Please respond to
TechNet E-Mail
Forum
<[log in to unmask]>
; Please respond
to
"Juan T. Marugán"
<[log in to unmask]
ES>
Thank you all for your suggestions,
Brian, the flux we are using is Alphametals 615-15 (ROL1) and I agree with
you that the best action will be prevention. But now, to change all the
connectors is not possible. So, we need to clean…
We have tried to carry out the method proposed by George and although it
works, we would like not add more rosin flux (the assembly is very complex)
We know that IPA is not the best solution but it is a standard product.
141-b can damage other parts of the unit (by the way, I suppose that our
company doesn’t purchase it in the black market) The new products
suggested by Brian should be qualified before use in the process, and
the “time flies”…
Brian, can you recommend us other solution (easy to purchase, not toxic
enough…)? I’m probably asking for a miracle.
Thank you again
Juan
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
|
|
|