TECHNET Archives

September 2005

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
TechNet E-Mail Forum <[log in to unmask]>, [log in to unmask]
Date:
Fri, 16 Sep 2005 07:33:47 -0400
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, "Scott B. Westheimer" <[log in to unmask]>
Subject:
MIME-Version:
1.0
Content-Transfer-Encoding:
7bit
Content-Type:
text/plain; format=flowed; charset="iso-8859-1"; reply-type=original
From:
"Scott B. Westheimer" <[log in to unmask]>
Parts/Attachments:
text/plain (156 lines)
You can check to see if the boards are actually under cured by perform Tg
analysis. Check for double pecks. I would be hesitant in accepting these
parts. If your supplier has a chart recorder on their press ask them for a
copy to see time at temperature and pressure. I would ask for replacement
and make sure that you check the date code so you can make sure that they do
not send you back the same boards.


Scott B. Westheimer
----- Original Message -----
From: "Steve Gregory" <[log in to unmask]>
To: <[log in to unmask]>
Sent: Friday, September 16, 2005 7:16 AM
Subject: Re: [TN] Rework for Delaminated PWBs


> Mornin' Everybody!
>
> I have the pictures that Mumtaz sent me posted now. Go to:
>
> http://www.stevezeva.homestead.com  and click on "Picture Page 2"
> and look at; "Blister 1, Blister 2, After Bake 1, and After Bake 2".
>
> Boy, that's some SERIOUS delamination! I don't know enough to say
> if the rework that your supplier is proposing is acceptable, but my first
> question would be is why would they send you boards that are not cured?
>
> If they sent you boards that are that undercured, what else is wrong with
> these boards?
>
> I would have a very hard time accepting these boards. Which brings up
> another question, if you say you won't accept them and that you want new
> boards, how will you know that you won't get the same boards that your
> supplier has "reworked"?
>
> Kind regards,
>
> -Steve Gregory-
> Senior Process Engineer
> LaBarge Incorporated
> Tulsa, Oklahoma
> (918) 459-2285
> (918) 459-2350 FAX
>
>
>
>
>                      Mumtaz Bora
>                      <mbora@KYOCERA-WI        To:
> [log in to unmask]@SMTP@Exchange
>                      RELESS.COM>              cc:       (bcc: Stephen R
> Gregory/LABARGE)
>                      Sent by: TechNet         Subject:  [TN] Rework for
> Delaminated PWBs
>                      <[log in to unmask]>
>
>
>                      09/15/2005 08:20
>                      PM
>                      Please respond to
>                      TechNet E-Mail
>                      Forum
>                      <[log in to unmask]>
>                      ; Please respond
>                      to Mumtaz Bora
>                      <mbora@KYOCERA-WI
>                      RELESS.COM>
>
>
>
>
>
> Dear Technetters,
>
>
> We have received a large batch of PWBs that is showing delamination after
> reflow at peak temp. 230C. Laminate is high Tg - 170C.
>
> Supplier is proposing to perform the following rework -- on these boards
> instead of providing replacement parts.
>
>  Oven bake at 190C for 2.5 hours followed by second bake at 150C for 2
> hours at 6kg/cm2 pressure. Will this guarantee a full cure?
>
> I am concerned about latent failures and layers opening up as full cure
> was
> not achieved the first time.
>
> Any inputs from the forum will be appreciated.
>
> I will request Steven Gregory to place the image of delamination on his
> website.  Have a great weekend.
> Thank-you
>
> Mumtaz
>
>  D/ 252 - SMT Process and Component Quality
>  Bldg. V238E
> Voice  (858)-882-1967
> Fax    (858)-882-3126
> Page  (858)-635-1180
> Cell:   (858) -449-7054
> email: [log in to unmask]
> Kyocera-Wireless Corp.
> 10300, Campus Point Drive
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 1.8e
> To unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt or (re-start) delivery of Technet send e-mail to
> [log in to unmask]: SET Technet NOMAIL or (MAIL)
> To receive ONE mailing per day of all the posts: send e-mail to
> [log in to unmask]: SET Technet Digest
> Search the archives of previous posts at: http://listserv.ipc.org/archives
> Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
> for additional information, or contact Keach Sasamori at [log in to unmask] or
> 847-615-7100 ext.2815
> -----------------------------------------------------
> San Diego, Ca  92121,USA
>
>
>
> __________________________________________________________________
> This message may contain information that is privileged and confidential
> to
> LaBarge, Inc.  It is for use only by the individual or entity named above.
> If you are not the intended recipient, you may not copy, use or deliver
> this message to anyone.  In such event, you should destroy the message and
> kindly notify the sender by reply e-mail.
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 1.8e
> To unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt or (re-start) delivery of Technet send e-mail to
> [log in to unmask]: SET Technet NOMAIL or (MAIL)
> To receive ONE mailing per day of all the posts: send e-mail to
> [log in to unmask]: SET Technet Digest
> Search the archives of previous posts at: http://listserv.ipc.org/archives
> Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
> for additional information, or contact Keach Sasamori at [log in to unmask] or
> 847-615-7100 ext.2815
> -----------------------------------------------------
>

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2