TECHNET Archives

August 2005

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Content-Type:
text/plain; charset="iso-8859-1"
Sender:
Subject:
From:
John Burke <[log in to unmask]>
Date:
Thu, 11 Aug 2005 13:49:30 -0700
MIME-Version:
1.0
X-To:
Cheryl Johnson <[log in to unmask]>, TechNet E-Mail Forum <[log in to unmask]>
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, John Burke <[log in to unmask]>
Parts/Attachments:
text/plain (468 lines)
For hard drives? is that the flex or the rigid board?

John
------------------------------------
Avanex
John Burke
Senior Manager RoHS Compliance
[log in to unmask]
40919 Encyclopedia Circle
Fremont
CA 94538
tel: 510 897 4250
fax: 510 979 0189
mobile: 510 676 6312
------------------------------------


-----Original Message-----
From: Cheryl Johnson [mailto:[log in to unmask]]
Sent: Thursday, August 11, 2005 1:49 PM
To: TechNet E-Mail Forum; John Burke
Subject: RE: [TN] <Misc>Re: [TN] <Misc>Re: [TN] RoHs board surface
recommendations.


Well I am a wife, don't have a tail (hair down to my waist, though...)
In any case, I have been using ENIG for several years with no problems.

HOWEVER, recently our off shore fab house is wanting us to go to "OSP over
copper".

Any comments?  Thank you!

Sincerely,
-----------------------------------
Cheryl Johnson, C.I.D.+
Manager
ExcelStor US Office, Engineering Services
Email: [log in to unmask]
Tel: (303) 684-7291
Fax: (303) 684-7268
Mobile: (303) 809-5815
-----------------------------------


-----Original Message-----
From: TechNet [mailto:[log in to unmask]]On Behalf Of John Burke
Sent: Thursday, August 11, 2005 1:16 PM
To: [log in to unmask]
Subject: Re: [TN] <Misc>Re: [TN] <Misc>Re: [TN] RoHs board surface
recommendations.


Yup.......................

Lets change the chemistry topic...............Ice cream anyone??

John

------------------------------------
Avanex
John Burke
Senior Manager RoHS Compliance
[log in to unmask]
40919 Encyclopedia Circle
Fremont
CA 94538
tel: 510 897 4250
fax: 510 979 0189
mobile: 510 676 6312
------------------------------------


-----Original Message-----
From: TechNet [mailto:[log in to unmask]]On Behalf Of Stadem, Richard
Sent: Thursday, August 11, 2005 1:09 PM
To: [log in to unmask]
Subject: Re: [TN] <Misc>Re: [TN] <Misc>Re: [TN] RoHs board surface
recommendations.


It must be Friday for some of us:)

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Chris Ball
Sent: Thursday, August 11, 2005 2:48 PM
To: [log in to unmask]
Subject: Re: [TN] <Misc>Re: [TN] <Misc>Re: [TN] RoHs board surface
recommendations.

......unnnnh........no tail.......wife..........must
resist.........arrrrgh....




                       Steve Hodge
                       <[log in to unmask]>           To:
[log in to unmask]
                       Sent by: TechNet                  cc:
                       <[log in to unmask]>                 Subject:    Re:
[TN] <Misc>Re: [TN]
                                                           <Misc>Re:
[TN] RoHs board surface
                       08/11/2005 03:36 PM
recommendations.
                       Please respond to TechNet
                       E-Mail Forum; Please
                       respond to Steve Hodge







George, I am sorry you feel you have to downgrade my opinion as being a
sales pitch or "wife's tail". I am stating data -substantiated facts and
I could care less about selling something to you or anyone else. A
wife's tail? What? My wife does not have a tail. I think it should be
"wive's tale" anyway.

At 12:30 PM 08/11/2005, you wrote:
>John,
>
>Your opinionated!  but then too so am I.  However, it sounds like our
>opinions are based on data and not "wife's tails" or "sales pitches"
>
>Regards,
>George
>George M. Wenger
>Reliability / FMA Engineer
>Base Station and Subsystems Group
>Andrew Corporation, 40 Technology Drive, Warren, NJ 07059 (908)
>546-4531 [log in to unmask]
>
>
>-----Original Message-----
>From: TechNet [mailto:[log in to unmask]]On Behalf Of John Burke
>Sent: Thursday, August 11, 2005 2:16 PM
>To: [log in to unmask]
>Subject: Re: [TN] <Misc>Re: [TN] RoHs board surface recommendations.
>
>
>Very nice,
>
>Until you consider that ENIG infringes the design rules for at least
>one
of
>the top 3 global CM's due to the issues associated with it.
>
>If you want the number of their chief technologist who has to look at
enigma
>failures week in week out I will happily supply details off line.
>
>I personally have built hundreds of thousands of assemblies on ENIG as
well
>as Immersion AG.
>
>As for the rest, HASL is generally failure related to a complete lack
>of understanding of tin thickness and intermetallic growth rate, OSP
>failures generally are related to not understanding the degradation of
>that finish with multiple reflow cycling, and personally I would never
>use immersion
tin
>without some type of diffusion barrier between it and the copper if nay
time
>in storage was to be considered.
>
>The ENIG when it fails can be catastrophic............and in most cases
can
>be pointed back to the process at the fab house rather than what
>happened
to
>it during the assembly process, unlike most of the other finish
>defects,
and
>has to my knowledge resulted in multi million dollar lawsuits between
>companies in the bay area due to failures.
>
>If it doesn't fail - it is fine, but the joint shear strength is less
>than the equivalent HASL or immersion AG finish due to the Tin
>nickel/nickel copper crystalline structure, so taking into
>consideration the higher temperatures of lead free I would be vary
>careful using it for area array packages using this soldering
technology.
>
>For the record have been using immersion silver since 1996 as I
>produced
the
>first beta site production runs using alpha level, so perhaps my views
have
>a little more history.
>
>Call me opinionated - I'll take it.
>
>John
>
>
>
>
>
>
>
>------------------------------------
>Avanex
>John Burke
>Senior Manager RoHS Compliance
>[log in to unmask]
>40919 Encyclopedia Circle
>Fremont
>CA 94538
>tel: 510 897 4250
>fax: 510 979 0189
>mobile: 510 676 6312
>------------------------------------
>
>
>-----Original Message-----
>From: Steve Hodge [mailto:[log in to unmask]]
>Sent: Thursday, August 11, 2005 10:44 AM
>To: TechNet E-Mail Forum; John Burke
>Subject: Re: <Misc>Re: [TN] RoHs board surface recommendations.
>
>
>John, come on now. Anything can happen at any time. I have seen some
>reservations from the IS users as to silver migration possibilities and

>shelf life/handling issues --you might say they have not seen them
--"yet".
>I have had more problems with HASL, OSP and IT than I have with ENIG.
>ENIG has longer data history than IS, so both shoes have already
>dropped so to speak. Three years without problems, is an eternity in
>this business, especially when we are expected to build  custom
products in 24 hours.
>
>
>At 11:00 AM 08/11/2005, you wrote:
> >with it............YET..........
> >
> >------------------------------------
> >Avanex
> >John Burke
> >Senior Manager RoHS Compliance
> >[log in to unmask]
> >40919 Encyclopedia Circle
> >Fremont
> >CA 94538
> >tel: 510 897 4250
> >fax: 510 979 0189
> >mobile: 510 676 6312
> >------------------------------------
> >
> >
> >-----Original Message-----
> >From: TechNet [mailto:[log in to unmask]]On Behalf Of Edwin Louis
> >Sent: Thursday, August 11, 2005 4:48 AM
> >To: [log in to unmask]
> >Subject: Re: [TN] RoHs board surface recommendations.
> >
> >
> >We have been using ENIG now for about three years and have had no bad

> >experiences with it. NASA for one does not allow the use of silver .
> >
> >-----Original Message-----
> >From: TechNet [mailto:[log in to unmask]] On Behalf Of Werner Engelmaier
> >Sent: Wednesday, August 10, 2005 4:57 PM
> >To: [log in to unmask]
> >Subject: Re: [TN] RoHs board surface recommendations.
> >
> >Hi Steve,
> >I do not know about "bad-mouth ENIG"--I am a reliability consultant,
> >and have had plenty of calls because of ENIG related failures, but
> >not a one
about
> >iAg. On the other hand, I do not know about their respective
environmental
> >implications.
> >
> >Regards,
> >Werner Engelmaier
> >Engelmaier Associates, L.C.
> >Electronic Packaging, Interconnection and Reliability Consulting
> >7 Jasmine Run
> >Ormond Beach, FL 32174 USA
> >Phone: 386-437-8747, Fax: 386-437-8737, Cell: 386-316-5904
> >E-mail: [log in to unmask], Website: www.engelmaier.com
> >
> >
> >---------------------------------------------------
> >Technet Mail List provided as a service by IPC using LISTSERV 1.8e To

> >unsubscribe, send a message to [log in to unmask] with following text
in
> >the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt

> >or (re-start) delivery of Technet send e-mail to
> >[log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing

> >per day of all the posts: send e-mail to
> >[log in to unmask]: SET Technet Digest
> >Search the archives of previous posts at:
http://listserv.ipc.org/archives
> >Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16
> >for additional information, or contact Keach Sasamori at
> >[log in to unmask]
or
> >847-615-7100 ext.2815
> >-----------------------------------------------------
> >
> >---------------------------------------------------
> >Technet Mail List provided as a service by IPC using LISTSERV 1.8e To

> >unsubscribe, send a message to [log in to unmask] with following text
in
> >the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt

> >or (re-start) delivery of Technet send e-mail to
> >[log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing

> >per day of all the posts: send e-mail to
> >[log in to unmask]: SET Technet Digest
> >Search the archives of previous posts at:
http://listserv.ipc.org/archives
> >Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16
> >for additional information, or contact Keach Sasamori at
> >[log in to unmask]
or
> >847-615-7100 ext.2815
> >-----------------------------------------------------
> >
> >---------------------------------------------------
> >Technet Mail List provided as a service by IPC using LISTSERV 1.8e To

> >unsubscribe, send a message to [log in to unmask] with following text
in
> >the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt

> >or (re-start) delivery of Technet send e-mail to
> >[log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing

> >per day of all the posts: send e-mail to
> >[log in to unmask]: SET Technet Digest
> >Search the archives of previous posts at:
http://listserv.ipc.org/archives
> >Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16
> >for additional information, or contact Keach Sasamori at
> >[log in to unmask]
or
> >847-615-7100 ext.2815
> >-----------------------------------------------------
>
>
>---------------------------------------------------
>Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
>unsubscribe, send a message to [log in to unmask] with following text in
>the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt
>or (re-start) delivery of Technet send e-mail to
>[log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing
>per day of all the posts: send e-mail to
>[log in to unmask]: SET Technet Digest
>Search the archives of previous posts at:
>http://listserv.ipc.org/archives Please visit IPC web site
>http://www.ipc.org/contentpage.asp?Pageid=4.3.16
>for additional information, or contact Keach Sasamori at [log in to unmask]

>or 847-615-7100 ext.2815
>-----------------------------------------------------
>
>-----------------------------------------------------------------------
>-------------------------

>This message is for the designated recipient only and may contain
>privileged, proprietary, or otherwise private information.
>If you have received it in error, please notify the sender immediately
>and delete the original.  Any unauthorized use of this email is
>prohibited.
>-----------------------------------------------------------------------
>-------------------------

>[mf2]
>
>---------------------------------------------------
>Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
>unsubscribe, send a message to [log in to unmask] with following text in
>the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt
>or (re-start) delivery of Technet send e-mail to
>[log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing
>per day of all the posts: send e-mail to
>[log in to unmask]: SET Technet Digest
>Search the archives of previous posts at:
>http://listserv.ipc.org/archives Please visit IPC web site
>http://www.ipc.org/contentpage.asp?Pageid=4.3.16
>for additional information, or contact Keach Sasamori at [log in to unmask]

>or 847-615-7100 ext.2815
>-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing
per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask]
or 847-615-7100 ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
archives of previous posts at: http://listserv.ipc.org/archives Please
visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2