Hi Karen,
You have gotten good advice so far.
The 'thermal stress' George is referring to, has to do with the thermal
expansion mismatch between the cermic chip and the PCB, and this in combination of
large solder fillets. The larger the fillets, the higher the stress. The
larger the pads, the larger the fillets. Also of course, the larger the delta-T,
the higher the stress. Thus, you will see more chip cracking with LF-solders.
The faster the heat transfer, both on heating and cooling, the higher the
thermal shock stress. On heating, wave soldering has the highest thermal shock.
Werner Engelmaier
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|
|
|