We have been manufacturing boards with immersion silver for 8 years, six
of those we have supplied plugged vias.
The process works best BEFORE the immersion silver process. It should not
be done after immersion silver because of the possibility of contaminating
the silver.
There NEVER should be anything in the via holes that could etch the hole
walls. They must have a very marginal via plugging process. Best pick
another fabricator until they improve their via plugging. Open vias could
increase assembly problems and cost you more money.
Happy Holden
Westwood Associates
Kanaiyalal Patel <[log in to unmask]>
Sent by: TechNet <[log in to unmask]>
06/10/2005 05:23 PM
Please respond to
TechNet E-Mail Forum <[log in to unmask]>; Please respond to
Kanaiyalal Patel <[log in to unmask]>
To
[log in to unmask]
cc
Subject
[TN] Immersion Silver - Via Plugging
Our supplier is recommending against plugging via holes the immersion
silver boards and here is their explanation. Need some input into how you
guys are managing.
"We can not plug before silver because chemicals used during the silver
process may become trapped. Over time these chemicals can eat away at the
hole wall copper creating voids.
2. Because the boards have passed through rout and are in piece form when
silver is applied the board can not be plugged in panel form as are the
gold boards.
3. Immersion silver is soft and easily damaged. It is our last
manufacturing process and we avoid handling it as much as possible after
being coated, this particularly applies for the plug process."
Appreciate your feedback.
re,
Hemant
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|
|
|