TECHNET Archives

May 2005

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
Date:
Fri, 13 May 2005 15:17:15 -0400
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, Bev Christian <[log in to unmask]>
Subject:
MIME-Version:
1.0
Content-Transfer-Encoding:
quoted-printable
Content-Type:
text/plain; charset="us-ascii"
From:
Bev Christian <[log in to unmask]>
Parts/Attachments:
text/plain (64 lines)
Werner,

I used the hokey expression of "intermittent micro-cracks" to waylay
people suggesting I use x-ray of one sort or another.  And, yes, I was
talking about a full crack across the entire SJ.  The problem with this
part is that it is so complex I am not sure that 100% functional testing
is possible.

Bev

RIM

 

  _____  

From: [log in to unmask] [mailto:[log in to unmask]] 
Sent: May 13, 2005 3:14 PM
To: [log in to unmask]; Bev Christian
Subject: Re: [TN] NDT Question

 

Hi Bev,
It sort of dependents. First there is no such thing as intermittent
micro-cracks in SJs. If they are micro-cracks, they can be present
starting about 40% into the life of the SJs, but they do not impact
electrical signals, intermittent or otherwise. If you have a full solder
joint fracture, electrical signal interruption will be intermittent,
because the fracture surfaces are in at least some slight compression
and make very good 'connector surfaces.'
If you have fully fractures SJs, they will only show intermittent opens
if they are disturbed by either temperature changes or mechanical
shock/vibration. The best way to find them is to do functional tests
during vibration loading.

Regards,
Werner Engelmaier
Engelmaier Associates, L.C.
Electronic Packaging, Interconnection and Reliability Consulting
7 Jasmine Run
Ormond Beach, FL 32174 USA
Phone: 386-437-8747, Fax: 386-437-8737, Cell: 386-316-5904
E-mail: [log in to unmask], Website: www.engelmaier.com







---------------------------------------------------------------------
This transmission (including any attachments) may contain confidential information, privileged material (including material protected by the solicitor-client or other applicable privileges), or constitute non-public information. Any use of this information by anyone other than the intended recipient is prohibited. If you have received this transmission in error, please immediately reply to the sender and delete this information from your system. Use, dissemination, distribution, or reproduction of this transmission by unintended recipients is not authorized and may be unlawful.

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2