Hi Paul,
The explanation you got for your BGA via failures does not sound right. Vias
fail because of the tension on the via barrel during high temperature
excursions, and the barrel copper not being good (thickness, strength, ductility) to
successfully resist this thermal expansion mismatch.
If forcing out too much resin during the lamination process, you get
delaminations, not voids; but reduced resin content actually reduces the thermal
expansion mismatch.
Regards,
Werner Engelmaier
Engelmaier Associates, L.C.
Electronic Packaging, Interconnection and Reliability Consulting
7 Jasmine Run
Ormond Beach, FL 32174 USA
Phone: 386-437-8747, Fax: 386-437-8737, Cell: 386-316-5904
E-mail: [log in to unmask], Website: www.engelmaier.com
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|
|
|