Bev: It depends. :>)
If you are using water soluble paste you should remove it as soon as
possible. The higher activity level of the flux starts to react with the OSP
coating.
If you are using no-clean it's not as critical. However we remove(wash)the
no-clean paste as soon as practical.
Also it's important that the boards are thoroughly dried after wash. You
don't want wet/damp boards sitting around with an OSP coating.
We've held boards for up to a month after washing paste and did not
experience any solderabilty or activation issues using ENTEK 106A+
Regards
Michael
Barmuta
Staff
Engineer
Fluke Corp.
Everett WA
425-446-6076
-----Original Message-----
From: TechNet [mailto:[log in to unmask]]On Behalf Of Bev Christian
Sent: Wednesday, May 11, 2005 9:51 AM
To: [log in to unmask]
Subject: [TN] Washing OSP boards
TechNetters,
If one were to wash misprinted OSP boards would it be worse to
a) leave the solder paste on 4 hours and then wash and use right away
or
b) wash right away and then let sit four hours before reprinting and
reflowing
I looked in the archives, but didn't find anything that was particularly
helpful.
This is a general question so I can't give solvent, wash time (and thus
amount of OSP left). So, Doug P., don't give me "it depends" as an
answer!
Bev
RIM
---------------------------------------------------------------------
This transmission (including any attachments) may contain confidential
information, privileged material (including material protected by the
solicitor-client or other applicable privileges), or constitute non-public
information. Any use of this information by anyone other than the intended
recipient is prohibited. If you have received this transmission in error,
please immediately reply to the sender and delete this information from your
system. Use, dissemination, distribution, or reproduction of this
transmission by unintended recipients is not authorized and may be unlawful.
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|
|
|