Vladimir Igoshev <[log in to unmask]>
Reply To:
TechNet E-Mail Forum <[log in to unmask]>, Vladimir Igoshev <[log in to unmask]>
Date:
Thu, 14 Apr 2005 12:33:09 -0400
Content-Type:
text/plain
Parts/Attachments:
text/plain (164 lines)
Hi Jim,

I'll have to search through my "archive", but there is a good technical summary from Atotech (a couple of years old, I believe), which compares "Black Pad" and "Brittle Fracture". I'll try to find out whether I can send it to you. The appearance of the fracture surface is identical for both cases, but the BF occurs only as a result of an impact type of loading and only on ENIG. 

Regards,

Vladimir

Vladimir Igoshev, Ph. D.
Senior Materials Researcher
Research in Motion
451 Phillip St.
Waterloo, ON, N2L 3X2

Voice: (+1) 519-888-7465, ext. 5283
Fax: (+1) 519-886-0863
E-mail: [log in to unmask]


-----Original Message-----
From: TechNet [mailto:[log in to unmask]]On Behalf Of Harold Kittel
Sent: Thursday, April 14, 2005 12:24 PM
To: [log in to unmask]
Subject: Re: [TN] ENIG - no more problems?


Vladimir,

Could you elaborate on this "Brittle Fracture" problem or possibly give some
references for me to investigate?  I have heard bits & pieces but not seen
any kind of a report.  I know Sandia Labs refers to "return of the Au" where
supposedly the gold initially dissolved into the solder diffuses back into
the solder/nickel interface to form an IMC layer.

Thanks,
Jim Kittel
L-3 Communications

-----Original Message-----
From: Vladimir Igoshev [mailto:[log in to unmask]]
Sent: Thursday, April 14, 2005 10:02 AM
To: [log in to unmask]
Subject: Re: [TN] ENIG - no more problems?


Well, I'm just wondering whether they have also sold the "Brittle Fracture"
problem, which ENIG is prone to. I'm seriously doubting that they have.


Vladimir

Vladimir Igoshev,
Research in Motion
451 Phillip St.
Waterloo, ON, N2L 3X2

Voice: (+1) 519-888-7465, ext. 5283
Fax: (+1) 519-886-0863
E-mail: [log in to unmask]


-----Original Message-----
From: TechNet [mailto:[log in to unmask]]On Behalf Of Genny Gibbard
Sent: Thursday, April 14, 2005 11:54 AM
To: [log in to unmask]
Subject: [TN] ENIG - no more problems?


Just listened to a Lead Free presentation by one of our assembly materials
suppliers.  They tested different pastes on different board finishes using a
variety of different patterns, spacings, aperture sizes, etc,...
By far and away, ENIG was the best finish for performance, for wetting,
defects, voiding, ...
The guy making the presentation said that he felt a lot of the initial
concerns re ENIG - black pad being the biggest - have been resolved, and
that they are no longer a concern, that they have determined what the cause
of it is and eliminated it.  Anyone want to comment on that?  I'm not sure
if he is correct, or just out of the loop.
It was interesting as well:  ImmAg got a very bad rating from them in
performance, even though many on this forum really praise that finish.  It
exhibited dewetting (they printed solderpaste pads on an area with no
soldermask, and the solder did not stay and spread where it was printed, it
crept together with other pads into a big blob, like you might see a water
drop do) and the amount of voiding was impressive!!
About 4 years ago I joined this forum, and one of the reasons was because I
was looking for info on ENIG.  We had done a prototype run of a couple of
boards and they failed miserably.  They were never analyzed in depth, so it
wasn't figured out what exactly caused the failure.  It was the excuse we
needed to not choose this finish and some of the extra costs associated with
it.
However, with the Pbfree push now, I don't know if we should re-examine
whether to use the finish.  For products where we needed a flat finish, we
have gone to ImmSn, but we still use HASL wherever possible.

Genny

"Genius may have its limitations, but stupidity is not thus handicapped"
Elbert Hubbard

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------



---------------------------------------------------------------------
This transmission (including any attachments) may contain confidential
information, privileged material (including material protected by the
solicitor-client or other applicable privileges), or constitute non-public
information. Any use of this information by anyone other than the intended
recipient is prohibited. If you have received this transmission in error,
please immediately reply to the sender and delete this information from your
system. Use, dissemination, distribution, or reproduction of this
transmission by unintended recipients is not authorized and may be unlawful.

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------



---------------------------------------------------------------------
This transmission (including any attachments) may contain confidential information, privileged material (including material protected by the solicitor-client or other applicable privileges), or constitute non-public information. Any use of this information by anyone other than the intended recipient is prohibited. If you have received this transmission in error, please immediately reply to the sender and delete this information from your system. Use, dissemination, distribution, or reproduction of this transmission by unintended recipients is not authorized and may be unlawful.

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2