Interesting, never heard of changing the electrical properties by baking
under cured FR-4.
If we had low peel or significant change in peel after solder float which
always also had low Tg we would bake the FR-4 for 10 to 12 hours at 345F.
If you have solder on these boards keep the temp below 310F and extend the
time, probably 24 hours. Best if you place a steel plate and some weight on
top of a stack of boards.
Have you had the Tg and UTg checked. If there is a gap in these numbers
greater than about 2 ppm the material is probably under cured.
I do not think you will get any additional cross linking of the resin until
above 285 F for a really long time. Days and days.
Good Luck
Chuck Brummer
Siemens
-----Original Message-----
From: Kaye Clayo [mailto:[log in to unmask]]
Sent: Wednesday, April 27, 2005 12:53 PM
To: [log in to unmask]
Subject: Re: [TN] How to Bake FR4 Boards
Judy
From what I understand, and that is not a lot, hook is when
Er changes with frequency at low frequencies, which changes
the capacitance, which results in distortion of output signals.
If anyone has any other information about this phenomenon,
please enlighten us.
Kaye
At 03:36 PM 4/27/2005, Judy Brown wrote:
>What is a "hook problem"?
>
> Judy
>
>-----Original Message-----
>From: TechNet [mailto:[log in to unmask]] On Behalf Of Kaye Clayo
>Sent: Wednesday, April 27, 2005 12:10 PM
>To: [log in to unmask]
>Subject: [TN] How to Bake FR4 Boards
>
>Dear Technet:
>
>Can someone tell me what temperature and duration
>we should bake some unpopulated FR4 (HASL) boards?
>
>We are attempting an experiment to see if we can "bake" a
>potential problem out of certain boards, but we don't know
>what the baking temperature / time should be. The potential
>problem we are looking to bake out is under cured laminate
>which could be causing a hook problem.
>
>Please help.
>
>Kaye
>
>
>CONFIDENTIALITY NOTE: This message is intended only for the use of the
>individual or entity to which it is addressed and may contain
>information that is privileged, confidential, and exempt from disclosure
>under applicable law. If the reader of this notice is not the intended
>recipient, you are hereby notified that any dissemination, distribution
>or copying of this communication is strictly prohibited. If you have
>received this communication in error, please notify the sender
>immediately.
>
>
>
>________________________________________________________________________
>_____
>Scanned by IBM Email Security Management Services powered by
>MessageLabs. For more information please visit http://www.ers.ibm.com
>________________________________________________________________________
>_____
>
>---------------------------------------------------
>Technet Mail List provided as a service by IPC using LISTSERV 1.8e
>To unsubscribe, send a message to [log in to unmask] with following text
>in
>the BODY (NOT the subject field): SIGNOFF Technet
>To temporarily halt or (re-start) delivery of Technet send e-mail to
>[log in to unmask]: SET Technet NOMAIL or (MAIL)
>To receive ONE mailing per day of all the posts: send e-mail to
>[log in to unmask]: SET Technet Digest
>Search the archives of previous posts at:
>http://listserv.ipc.org/archives
>Please visit IPC web site
>http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
>information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
>ext.2815
>-----------------------------------------------------
>
>___________________________________________________________________________
__
>Scanned by IBM Email Security Management Services powered by MessageLabs.
For more information please visit http://www.ers.ibm.com
>___________________________________________________________________________
__
CONFIDENTIALITY NOTE: This message is intended only for the use of the
individual or entity to which it is addressed and may contain information
that is privileged, confidential, and exempt from disclosure under
applicable law. If the reader of this notice is not the intended recipient,
you are hereby notified that any dissemination, distribution or copying of
this communication is strictly prohibited. If you have received this
communication in error, please notify the sender immediately.
____________________________________________________________________________
_
Scanned by IBM Email Security Management Services powered by MessageLabs.
For more information please visit http://www.ers.ibm.com
____________________________________________________________________________
_
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|