TECHNET Archives

April 2005

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
TechNet E-Mail Forum <[log in to unmask]>, [log in to unmask]
Date:
Mon, 25 Apr 2005 14:56:17 -0400
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, Vladimir Igoshev <[log in to unmask]>
Subject:
MIME-Version:
1.0
Content-Transfer-Encoding:
quoted-printable
Content-Type:
text/plain; charset="iso-8859-1"
From:
Vladimir Igoshev <[log in to unmask]>
Parts/Attachments:
text/plain (71 lines)
Hello Victor,

I use 1 micron diamond suspension (for a "final touch") and it has always worked for me.

Vladimir

Vladimir Igoshev, Ph. D.
Senior Materials Researcher
Research in Motion
451 Phillip St.
Waterloo, ON, N2L 3X2

Voice: (+1) 519-888-7465, ext. 5283
Fax: (+1) 519-886-0863
E-mail: [log in to unmask]


-----Original Message-----
From: TechNet [mailto:[log in to unmask]]On Behalf Of Victor G. Hernandez
Sent: Monday, April 25, 2005 2:48 PM
To: [log in to unmask]
Subject: [TN] Lead Free, Ball Grid Array, solder bump cross section


Fellow TechNetters:

   I have conducted many of LF solder bump cross section and final
polish is conducted with a Buehler Masterprep

Polishing Suspension Alumina 0.05 microns.   Micro craves, epoxy
shrinkage/voids, on the sample surface retain

the polishing compound which contaminate the surface appearance.   This
step can cause staining and/or water

marks on the bulb solder prior to mid range magnification examination
with inverted stage microscope.

   Can some one recommend a LF chemical etchant that I can replace the
alumina step in my process? 

Victor,

 


---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------



---------------------------------------------------------------------
This transmission (including any attachments) may contain confidential information, privileged material (including material protected by the solicitor-client or other applicable privileges), or constitute non-public information. Any use of this information by anyone other than the intended recipient is prohibited. If you have received this transmission in error, please immediately reply to the sender and delete this information from your system. Use, dissemination, distribution, or reproduction of this transmission by unintended recipients is not authorized and may be unlawful.

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2