Hi George! Tin is not commonly used for contact services unless the
application uses high contact forces/pressures and the number
"insertions/dissertions" is minimal. Tin oxides are brittle and can "spall"
loose creating contact surface debris which usually results in intermittent
contact problems. The old IPC-GH-850 Guidelines document has a good section
on tin (as does the Volume 4 Materials reference). Tin also can have the
"tin whisker" problem which is driving a fair share of the industry nuts
right now. Silver seems to have a pretty bad reputation as a contact
surface due to use environment reactions. Silver oxide is as conductive as
elemental silver (which a pretty cool material characteristic) but
formation of silver sulfide results in significant electrical property
changes. Electrolytic silver also has the reputation for creating
electrical traces that a designer doesn't want - pretty high incidence of
electrochemical migration problems in some use environments. The
military/high rel folks banned the use of silver as a contact material many
years ago. You might investigate the possible use of the new immersion
silver or immersion gold chemistries to see if they could be used in your
application. Both plating systems are being used with great success on pwbs
(which you already know!). If your current use of tin isn't having any
spalling or fretting corrosion issues, you may already have an optimum
material set. Good Luck.
Dave
"Wenger, George
M."
<George.Wenger@AN To
DREW.COM> [log in to unmask]
Sent by: TechNet cc
<[log in to unmask]>
Subject
Re: [TN] Microcircuit Palladium
03/02/2005 06:18 Lead Finish (Good or Bad)?
PM
Please respond to
TechNet E-Mail
Forum
<[log in to unmask]>
; Please respond
to
"Wenger, George
M."
<George.Wenger@AN
DREW.COM>
David,
Now that you have your connector handbook open could I ask if you would
check to see if there is any information about the use of silver and tin
as matting surfaces. I have a toggle switch that has a yellow brass
movable contact with a silver button that contacts a tin plated copper
button on the stationary side of the contact. Historically we avoid the
use of gold and tin as matting surface because of the galvanic potential
between the two materials and the possibility of fretting corrosion but
I don't remember seeing any information concerning silver and tin
Regards,
George
George M. Wenger, Andrew Corporation
Reliability / FMA Engineer
Base Station & Subsystems Group
40 Technology Drive, Warren, NJ 07059
(908) 546-4531 [log in to unmask]
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of David D. Hillman
Sent: Wednesday, March 02, 2005 7:03 PM
To: [log in to unmask]
Subject: Re: [TN] Microcircuit Palladium Lead Finish (Good or Bad)?
Hi folks! Wow, what a way to named - "the guy who cuts up his water
pipes"! Well, its better than Doug's "It depends"! I do have some
information that might be helpful - the following info is taken from
Volume
4 Materials of the Connectors and Interconnections Handbook published by
the Electronic Connector Study Group Inc. (sorry, no ISBN available)
which
is a really good resource on connector materials.
- Pd wears better than Au for an equal plating thickness and can provide
an
adequate end of life contact
- Pd is somewhat less galvanically active toward copper and nickel than
corresponding deposits of either Au or rhodium
- 60Pd40Ag is recognized as a good contact material for industrial and
telecommunications applications
- Pd can tarnish due to sulfur contributing sources
- Pd can form frictional polymer in sliding contact applications that
are
exposed to organic vapors. The frictional polymer can increase contact
resistance.
I would recommend that you talk to the folks at Tyco or the J.M. Ney
Company - a Pd finish is being used widely in electronics applications
and
you just need to confirm that your application/use environment is
appropriate. Good Luck.
Dave Hillman
Rockwell Collins
[log in to unmask]
Charles Caswell
<CharlesC@FESCORP
.COM>
To
Sent by: TechNet [log in to unmask]
<[log in to unmask]>
cc
Subject
02/28/2005 06:33 Re: [TN] Microcircuit Palladium
AM Lead Finish (Good or Bad)?
Please respond to
TechNet E-Mail
Forum
<[log in to unmask]>
; Please respond
to
Charles Caswell
<CharlesC@FESCORP
.COM>
I don't have the spec available but I would think that Palladium finish
in
a
gold socket would be fine. I would not want to solder directly to
Palladium
however. Maybe Dave ( the guy who cuts up water pipes from his house! )
could
give us some insight.
-----Original Message-----
From: - Bogert [mailto:[log in to unmask]]
Sent: Friday, 25 February 2005 5:06 PM
To: [log in to unmask]
Subject: [TN] Microcircuit Palladium Lead Finish (Good or Bad)?
February 25, 2005
MIL-PRF-38535 microcircuit specification is confusing since in one
section
it
identifies that to select a lead finish, include a suffix letter as part
of
the part number. The available suffix letters are Finish "A", "B",
"C":,
"D"
and "X". "D" is for Palladium. "X" means either "A", "B", or "C"
Finish
However, Appendix A of the specification indicates that only lead
Finishes
"A" through "C" (or "X") are allowed.
It appears that Finish "D", Palladium finished microcircuit leads are
not
allowed. Is this true? If so, why the apparent prohibition on
Palladium
lead finish?
The question relates to selecting the lead finish for a microcircuit
that
is
mounted in a socket having Gold-plated socket contacts. Normally, one
should
specify a Gold-plated microcircuit lead (Finish "C") to mate with the
Gold-plated socket contact. However, from a galvanic corrosion
standpoint,
either Gold or Palladium should be ok.
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask]
or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask]
or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
------------------------------------------------------------------------------------------------
This message is for the designated recipient only and may
contain privileged, proprietary, or otherwise private information.
If you have received it in error, please notify the sender
immediately and delete the original. Any unauthorized use of
this email is prohibited.
------------------------------------------------------------------------------------------------
[mf2]
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|