TECHNET Archives

January 2005

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
TechNet E-Mail Forum <[log in to unmask]>, John Parsons <[log in to unmask]>
Date:
Thu, 13 Jan 2005 11:34:42 -0500
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, "Wenger, George M." <[log in to unmask]>
Subject:
MIME-Version:
1.0
Content-Transfer-Encoding:
quoted-printable
Content-Type:
text/plain; charset="iso-8859-1"
From:
"Wenger, George M." <[log in to unmask]>
Parts/Attachments:
text/plain (127 lines)
John,

You might want to check the final report from the NCMC PWB Surface Finsh Project that I thnk was completed in the 1998-1999 time period.  I think the 15u' minimum may come from an IBM specification that called for a 22u" average +/- 3sigma and if my memory is corect the standard deviation we were experiencing was in the 2.2u" range.

Regards,
George

George M. Wenger (908)-546-4531 
Reliability / FMA Engineer
Base Station and Subsystems Group
Andrew Corporation,  40 Technology Drive, Warren, NJ 07059
[log in to unmask]



-----Original Message-----
From: TechNet [mailto:[log in to unmask]]On Behalf Of John Parsons
Sent: Thursday, January 13, 2005 11:26 AM
To: [log in to unmask]
Subject: Re: [TN] FAB - Al Wire Bonding


 Thank you all for your input.  Basically you have confirmed what I was
initially told.  Now the question becomes where the 15u" spec came from.  I
have got the customer thinking about this as well and hope to hear back from
them today.  I am hoping that we can convert them to immersion gold and save
a bunch of fuss.  My calling the contacts "edge fingers" may have been a
misnomer, but they are fingers on the edge of the board :) .  They are
5x33mil pads at 9mil centers.  The customer is definitely wire bonding to
them so hard gold is not required.

Regards
John
-----Original Message-----
From: TechNet [mailto:[log in to unmask]]On Behalf Of Joyce Koo
Sent: Thursday, January 13, 2005 7:45 AM
To: [log in to unmask]
Subject: Re: [TN] FAB - Al Wire Bonding

are you guys sure it is connector? not leadframe?
                              jk

-----Original Message-----
From: TechNet [mailto:[log in to unmask]]On Behalf Of Jeffrey Bush
Sent: Thursday, January 13, 2005 7:59 AM
To: [log in to unmask]
Subject: Re: [TN] FAB - Al Wire Bonding


Connector fingers should be plated with harder gold - Knoop over 130.
Bondable gold is either AL or AU/Ball bonding.  In AL wire bonding the
bond is to the under plate of NI.  Some are successful at bonding the
electroless NI, but most are not.  Electrolytic NI seems to offer the
best reliability.  In this case I would call for a thin coating of soft
AU (17 uinches max), as the bonding action scrubs the protective AU
coating away to reach the NI layer.  Thicker gold will create bonding
issues for AL wire bond.  Using the thinner gold may also allow you to
go full body gold (for soldering also) and depending on the geometry of
the circuit is could be more economical that using selective gold
plating.  The electrolytic NI plating should be 118 uinches min.


Jeffrey Bush
Director, Quality Assurance and Technical Support

VERMONT CIRCUITS INCORPORATED
  76 Technology Drive - POB 1890
    Brattleboro, Vermont 05302
      Voice: 802.257.4571.21 Fax: 802.257.0011
           http://www.vtcircuits.com


-----Original Message-----
From: John Parsons [mailto:[log in to unmask]]
Sent: Wednesday, January 12, 2005 6:32 PM
To: [log in to unmask]
Subject: [TN] FAB - Al Wire Bonding

Greetings all,
I am trying to learn something about the wire bonding process.  Our
customer
has a part on which they spec the finish of some edge connector fingers
as
"Gold Plated for Wire Bonding Al Wire".  As we do not provide a wire
bondable gold finish in-house we have subcontracted the service.  The
plating service tells me that typically for Al wire bonding all that is
required is a typical ENIG process (5-10u" Au over 200u" Ni).  I believe
that in past verbal communications with the customer they have said that
an
ENIG finish would not suffice and that they require 15u" of bondable
gold
(electroless gold or electroplated??) .

What say you? Or does "it depend" :-)

Regards
John Parsons

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

------------------------------------------------------------------------------------------------
This message is for the designated recipient only and may
contain privileged, proprietary, or otherwise private information.  
If you have received it in error, please notify the sender
immediately and delete the original.  Any unauthorized use of
this email is prohibited.
------------------------------------------------------------------------------------------------
[mf2]

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2