TECHNET Archives

December 2004

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Content-Type:
text/plain; charset="iso-8859-1"
Sender:
Subject:
From:
"Ingemar Hernefjord (KC/EMW)" <[log in to unmask]>
Date:
Tue, 28 Dec 2004 14:08:03 +0100
MIME-Version:
1.0
X-To:
TechNet E-Mail Forum <[log in to unmask]>, "Brooks,Bill" <[log in to unmask]>
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, "Ingemar Hernefjord (KC/EMW)" <[log in to unmask]>
Parts/Attachments:
text/plain (188 lines)
Bill,

forgot to tell you that Joe Fjelstad has lots of information about LCP.
May be the coming new RF board material..

Ingemar


-----Original Message-----
From: Ingemar Hernefjord (KC/EMW)
Sent: den 28 december 2004 12:41
To: 'TechNet E-Mail Forum'; 'Brooks,Bill'
Subject: RE: [TN] Wanted: TN's best-on-coax-soldering



Quite right, Bill,

System is around 60 GHz, while the port you saw carries an intermediate frequency. But even that one is high enough to cause problems. Connector is lossy SMA, but we use other connectors for high performance, e.g. Rosenberger SMP, which is specified for 40 GHz, but useful much higher. Yes, 60 GHz   is not on ordinary lossy Duroid. Heard of LCP? Useful up to 100 GHz.

Ingemar


-----Original Message-----
From: TechNet [mailto:[log in to unmask]]
Sent: den 22 december 2004 18:46
To: [log in to unmask]
Subject: Re: [TN] Wanted: TN's best-on-coax-soldering


Ingemar,

I have not worked at 60GHz yet... The highest frequency I have worked at is
15Ghz. At 60GHz you are really in need of a waveguide-like connection I
would think... just intuition... What we were able to do at 3 to 6 GHz falls
apart as you get past 15GHz. What type of connector are they using? SSMA?
What substrate materials are being used?

Perhaps a short length of coaxial 'tail' on the back end of the connector
with a bend in it to allow for expansion and contraction and then some sort
of impedance matching network at the board launch site would work...

 I would love to see the packaging of this design... It would be very
enlightening to get a sense of scale too... I would expect 60GHz circuits to
be on some sort of a MMIC or chip... not at the board level... I would think
Duroid materials might still be too lossy at those frequencies.

Sounds like a terrific design challenge... what an opportunity to get into
cutting edge design... I envy you. :)

Best regards,


Bill Brooks - KG6VVP
PCB Design Engineer , C.I.D.+, C.I.I.
Tel: (760)597-1500 Ext 3772 Fax: (760)597-1510
e-mail:[log in to unmask]
http://www.dtwc.com
http://pcbwizards.com


-----Original Message-----
From: Ingemar Hernefjord (KC/EMW) [mailto:[log in to unmask]]
Sent: Wednesday, December 22, 2004 12:04 AM
To: 'TechNet E-Mail Forum'; 'Brooks,Bill'
Subject: RE: [TN] Wanted: TN's best-on-coax-soldering



Bill,
right about silver ribbon (I'd prefer gold). Theoretically best solution. I
proposed parallel gap welded ribbon with mini S-curve to take movements, but
does not work at 60 GHz range. Feel like don Q when fighting with the
microwave experts, my design-for-reliability proposals are overrun by
we-must-not-distort-the-signal guys...but after the environmental tests I
use to get visits from same guys, now ready to discuss reality...ho-ho

Thanks for your engagement

Ingemar


-----Original Message-----
From: TechNet [mailto:[log in to unmask]]On Behalf Of Brooks,Bill
Sent: den 17 december 2004 21:50
To: [log in to unmask]
Subject: Re: [TN] Wanted: TN's best-on-coax-soldering


Hi Steve,

Very interesting photo, do you have more from different perspectives?
The soldermask 'dam' is a great example of a technique I used at another
company.

The 'coined' or flattened lead from the SMA looks to be pulled away from the
solder joint... I would guess this happened after a thermal excursion, where
the chassis expanded faster than the board and the lead literally pulled the
SMA pin loose from the solder connection.

I can't tell a lot from the photo because of the frosted Plexiglas
appearance surrounding the top of the photo, but I have see this sort of
failure before in similar situations...

The solution to the problem is to strain relief the connection.
We used a silver ribbon and soldered it to the pin and the board allowing it
to flex to take up the CTE mismatch between the aluminum housing and the
Duroid board.

Hope that helps... let me know if I read the problem correctly... it was
just a guess based on what it looks like to me from here... not being able
to see the whole picture...

Best regards,

Bill Brooks - KG6VVP
PCB Design Engineer , C.I.D.+, C.I.I.
Tel: (760)597-1500 Ext 3772 Fax: (760)597-1510
e-mail:[log in to unmask]
http://www.dtwc.com
http://pcbwizards.com


-----Original Message-----
From: Steve Gregory [mailto:[log in to unmask]]
Sent: Friday, December 17, 2004 12:35 PM
To: [log in to unmask]
Subject: Re: [TN] Wanted: TN's best-on-coax-soldering

Sorry Everyone! My bad, I didn't have the thumbnail linked to the
picture...but it is now. Try this link:

http://www.stevezeva.homestead.com/files/SMA.jpg

Just got in a hurry when I posted the picture. I'm trying to get all my
loose ends tied-up here at work because I'm leaving this weekend for
Christmas vacation.

-Steve Gregory-

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2