Since the tensile strength of the copper plating is relational to the
thickness of the plating, it appears that the failure mode is a thin
area of plating in the via that could not support the z-axis expansion
and failed. Poor solution flow in the via can cause this - debris/poor
solution movement/poor throwing power to the low current density areas
can contribute.
Jeffrey Bush
Director, Quality Assurance and Technical Support
76 Technology Drive - POB 1890
Brattleboro, Vermont 05302
802.257.4571.21
http://www.vtcircuits.com
-----Original Message-----
From: paul reid [mailto:[log in to unmask]]
Sent: Friday, November 05, 2004 11:31 AM
To: [log in to unmask]
Subject: Re: [TN] Via hole failures (with pictures)
I believe you are looking at a barrel crack in the middle of a plated
through via (PTV). This is a typical failure mode from "Z" axis
expansion
of the material due to thermal excursions. The thermal excursions of
assembly/rework could induce this failure mode. Fabrication variables
like
copper thickness/quality or the type of material used in fabrication
could
be contributing factors. It is possible that a couple of those dark
lines
on the right side (middle and bottom) of the PTV in your picture are of
material delamination.
Paul Reid
PWB Interconnect Solutions Inc.
-----Original Message-----
From: Al Onderick [mailto:[log in to unmask]]
Sent: Thursday, November 04, 2004 5:55 PM
To: [log in to unmask]
Subject: [TN] Via hole failures (with pictures)
I have a couple of boards that have failed at a customer site. After
testing, a via was identified as open. The following link is a picture
of
the cross section.
http://www.tier1gear.com/temp/via_crack.jpg
The board was .062, the via .010 and the surface finish immersion white
tin.
I would appreciate any insight into what may cause a failure like this.
Al Onderick
National Instruments
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask]
or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|
|
|