What kind of etch are you using on your microsections? A statement from our
lab people "The lines were almost impossible to see under magnification using
ammonia/peroxide etch but were visible when chromic acid etch was used. But we
did not see corner cracks on coupons with demarcation lines when the panels
were plated in standard vertical tanks."
Also "Sounds like the "banded" deposit could be from a horizontal plater,
maybe
using inert anodes. These systems typically require higher brightener
content leading to poorer physical properties (cracks)."
Hope this helps track down the cause -
Denny Fritz
MacDermid.
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------