The testing that we have done with RPP does not have demarcation lines -
the reverse pulse just creates a slight de-plate current to level out
surface to hole ratios. All of our testing show a continuous copper
layer, but we have only tested a few sample types. I know that a
variety of rectifiers exist for RPP and possible this is the difference
- or malfunction of a unit/flight bar connection.
Jeffrey Bush
Director, Quality Assurance and Technical Support
76 Technology Drive - POB 1890
Brattleboro, Vermont 05302-1890
Tel. 802.257.4571.21 Fax. 802.257.0011
[log in to unmask]
http://www.vtcircuits.com
-----Original Message-----
From: Susan Mansilla [mailto:[log in to unmask]]
Sent: Friday, October 01, 2004 11:51 AM
To: [log in to unmask]
Subject: [TN] Pulse Plating
Greetings everyone,
I have two customers, both of whom use pulse plating to fabricate
boards. One has a continuous copper deposit and the other has multiple
bands or layers of plating - very visible after microetch.
The plating deposit on the banded product has cracks after Thermal
Stress.
In my limited experience I have not seen pulse plating result in such
definite bands.
My question is - would bands be expected and "normal" in some pulse
plating operations?
Thanks for your help
Susan Mansilla
Robisan Lab
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
archives of previous posts at: http://listserv.ipc.org/archives Please
visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------
|
|
|