Daan's assessment sounds right. This could have been a paste dry out
issue.
Jason, do you know what the metal % was in each of these solder pastes?
Best regards,
David Suraski
AIM
-----Original Message-----
From: Jason Gregory [mailto:[log in to unmask]]
Sent: Wednesday, October 27, 2004 9:08 AM
To: [log in to unmask]
Subject: Re: [TN] Question about 2% Ag and stencil release
Yes, same flux in both pastes
Jason Gregory
Manufacturing Engineer
Innova Electronics
(281)653-5593
(281)653-5594 fax
(281)310-7588 cell
[log in to unmask]
-----Original Message-----
From: TechNet [mailto:[log in to unmask]]On Behalf Of Taheri, Kamran
Sent: Tuesday, October 26, 2004 7:39 PM
To: [log in to unmask]
Subject: Re: [TN] Question about 2% Ag and stencil release
Jason, did both solder pastes have the same flux chemistry?
-----Original Message-----
From: TechNet [mailto:[log in to unmask]]On Behalf Of Daan Terstegge
Sent: Tuesday, October 26, 2004 4:00 PM
To: [log in to unmask]
Subject: Re: [TN] Question about 2% Ag and stencil release
Hi Jason,
I don't believe this has anything to do with silver.
The fine powder of your type 5 paste has a MUCH larger ratio between
soldersurface and soldervolume than the part 3 type, which means that it
is more difficult to keep the powder particles stable and oxide-free.
The smaller process window increases the chance of printing problems.
Hopefully a more accurate description will be given by one of the paste
manufacturers on this forum, but I think I'm pretty close....
Best regards,
Daan
http://www.smtinfo.net
----- Original Message -----
From: "Jason Gregory" <[log in to unmask]>
To: <[log in to unmask]>
Sent: Tuesday, October 26, 2004 9:44 PM
Subject: [TN] Question about 2% Ag and stencil release
> Has anybody had any experience or seen/written studies involving 2% Ag
> release from stencil apertures? We have a stencil, parts are small
resnets,
> about 15 mil pitch on a .006" thick stencil. Tried 2% silver paste
> (for tombstoning of other parts) with type 5 powder and had major
> release problems. We kept the same parameters on the screen printer
> (for reference/control purposes) and swapped in our "normal" 63/37
> Type 3
powder
> and release issues "virtually" went away. Not all the way, but for the
most
> part. I thought smaller mesh should have meant better release. Solder
> gurus ------- enlighten me!
>
> Jason Gregory
> Manufacturing Engineer
> Innova Electronics
> (281)653-5593
> (281)653-5594 fax
> (281)310-7588 cell
> [log in to unmask]
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
> unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt
> or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
> To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
> Search the archives of previous posts at:
> http://listserv.ipc.org/archives Please visit IPC web site
> http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask]
or 847-615-7100 ext.2815
> -----------------------------------------------------
>
>
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing
per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask]
or 847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing
per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask]
or 847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
archives of previous posts at: http://listserv.ipc.org/archives Please
visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|