Hi 'jk,'
The composite CTE of the PCB is important--at least as a sanity check, and of
course, the lay-up and lamination details are very important.
However, for PCBs during soldering processes and in severe operational
environments that is not enough. The only way to determine the local loading
conditions is to run FEA simulations--and these are only as good as the input
paramaters used; in fact, the can be useless or even misleading, unless the best
possible information is used.
In fact, there are 3 types of resin layers in any PCB: 'laminate' layers,
'prepreg' layers, and 'just' resin layers. This is important, because these
layers have diifferent properties; and because it has been observed over and over
again, that barrel cracks occur where the 'prepreg' layers are in the PCB.
The reason is clear; 'prepreg' layers have a significantly higher resin
content than 'laminate' layers and are also less fully cured. That results in a
higher CTE(z) for the 'prepreg' layers--I estimate that 'prepreg' layers have a
CTE(z, <Tg) ~10 to 15 ppm/C higher than the 'laminate' layers.
The 'just' resin layers are not x,y-constrained and thus have the isotropic
CTEs of the resin in all directions, but because they are thin, do not have any
real impact.
I received the information I need direct from Nelco.
N4000-13
X axis CTE (-40 to +125C.)=16.9 ppm/°C
Y axis CTE (-40 to +125C.)=4.9 ppm/°C
Z axis CTE (below Tg)=69ppm/°C
Z axis CTE (above Tg)=283ppm/°C
This is, I am quite certain, for 'laminate' layers. For 'prepreg' layers I
would estimate CTE(x,y) to be about the same, but Z axis CTE (below Tg)~79ppm/°C
and Z axis CTE (above Tg)~298ppm/°C. For the 'just' resin layers CTE (x/y/z,<
Tg)~30ppm/°C and CTE (x/y/z,>Tg)~100ppm/°C.
Regards,
Werner Engelmaier
Engelmaier Associates, L.C.
Electronic Packaging, Interconnection and Reliability Consulting
7 Jasmine Run
Ormond Beach, FL 32174 USA
Phone: 386-437-8747, Fax: 386-437-8737, Cell: 386-316-5904
E-mail: [log in to unmask], Website: www.engelmaier.com
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------
|