TECHNET Archives

October 2004

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Show All Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Subject:
From:
Daan Terstegge <[log in to unmask]>
Reply To:
TechNet E-Mail Forum <[log in to unmask]>, Daan Terstegge <[log in to unmask]>
Date:
Mon, 11 Oct 2004 11:13:11 +0200
Content-Type:
text/plain
Parts/Attachments:
text/plain (125 lines)
Hi Joe,

It could be that I don't understand the IPC well enough due to the fact
English is not my native language, but for me the IPC-A-610 says
"entrapped balls that are smaller than 0.13 mm are process indicators"
and "solder balls that are not entrapped or encapsulated (no matter
their size) are defects" .
This corresponds well with the ANSI-J-STD001C that mentions "Solder
balls or other metal particles shall neither be loose (i.e., be
dislodged in the normal service environment of the product) nor violate
minimum electrical clearance." Again I would make the interpretation as
"loose solder balls, no matter how small, are defects".





Best regards,

Daan Terstegge
PCB Assembly Department
Thales Land & Joint Systems

Tel +31(0)35 524 8297
Fax +31(0)35 524 8181
[log in to unmask]
Unclassified Email

>>> [log in to unmask] 10/08/04 05:55pm >>>
Hi Group,
Solder balls that are smaller than 0.13 mm (0.005 inch) and less than 5
per
600 mm squared (0.93 sq inch) are process indicators. If greater than
0.13
mm and not entrapped then it would be a defect. By entrap it usually
means
solder balls are trapped in no clean flux or in adhesives of some sort
or
tacked on to a conductor but not creating a clearance violation.

  Joe Bruce
  Functional Excellence
  Solectron - Winnipeg
  204 631-7233

Confidentiality Notice: This e-mail message, including any attachments,
is
for the sole use of the intended recipient(s) and may contain
confidential
and privileged information. Any unauthorized; review, use, disclosure
or
distribution is prohibited. If you are not the intended recipient,
please
contact the sender by reply e-mail and destroy all copies of the
original
message.



-----Original Message-----
From: Tom Moore [mailto:[log in to unmask]]
Sent: Friday, October 08, 2004 9:36 AM
To: [log in to unmask]
Subject: [TN] Solder balls acceptance criteria


Dear Group,
I'm asking the group again to impart your communal wisdom in
interpreting
IPC-A-610. We are seeing solder balls on our SMT assemblies after they
have
gone thru board wash (dishwasher). Would these be classified as
entrapped/encapsulated and therefore process indicators and not
subject
to "rework" (as long as they don't violate minimum electrical
clearance)?
Thanks.

Tom Moore

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask]
or
847-509-9700 ext.5315
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
ext.5315
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------

ATOM RSS1 RSS2