Hello Steve and Ingemar, I have some important news about the problem!
This corrosion happens too when the lead frames are only Ag without Pt, so
we can discard the Pt. But most significantly is the fact that this
phenomenon comes to view before the duration tests.
After the hybrids are produced (the bonding is still not made), they are
stored in trays. These trays are put one on the another forming little
columns. When the storage time is long (sorry, I can not cuantifize how many
days), the spots appears but only in the hybrids placed in the borders of
the trays. We have soldered the bonding wire on these hybrids and they works
perfectly, so the problem is only of external appereance.
I think that the cause is the typical slow reaction of silver with sulphur
that leads to Ag2S. This reason is the same that makes "dirty" the silver
crockery, but the spots are red not black. I include a photo of the device
to make my explanations easier to understand.
Thank you all for your help!
Best regards
Jose
-----Mensaje original-----
De: TechNet [mailto:[log in to unmask]]En nombre de Creswick, Steven
Enviado el: jueves, 26 de agosto de 2004 12:00
Para: [log in to unmask]
Asunto: Re: [TN] Corrosion in lead frames
Jose,
To the best of my knowledge, Pt will not oxidize with a red color.
I don't recall ever seeing such a condition develop. Approximately how
large are the red spots? Do they run up and down the edges of the
conductor, or are they all across the surface of the conductor? Are they on
the ceramic as well? Are they just in areas where flux has been?
How hot, and how long does it take for the spots to develop?
More questions than answers ...
Steve
-----Original Message-----
From: Jose Antonio Garcia Ontalba [mailto:[log in to unmask]]
Sent: Wednesday, August 25, 2004 1:21 PM
To: [log in to unmask]
Subject: Re: [TN] Corrosion in lead frames
Steve,
You are right, I am speaking of an alumina substrate with a Ag/Pt
metallization, but I have just realized that I was wrong in my first
message: the lead frame is really Ag/Pt and the coating is pure Ag. There is
not more metalls involved.
I think the red spots are oxides of Ag or Pt or maybe both. But the oxides
of silver are not red coloured, aren't they? So, the red spots have to be
oxides of Pt... Maybe the tempeature helps the reaction of oxidation of Pt.
Anyway I am not sure.
What do you think?
Thank you very much!
Regards
Jose
-----Mensaje original-----
De: TechNet [mailto:[log in to unmask]]En nombre de Creswick, Steven
Enviado el: miércoles, 25 de agosto de 2004 18:02
Para: [log in to unmask]
Asunto: Re: [TN] Corrosion in lead frames
Jose,
Could the red-orange color be from exposed, oxidized copper?
You did not say whether the lead frame was copper, phosphor bronze, or maybe
a Kovar (Fe, Ni, Co) composition.
.... although, I am confused by a lead frame having Ag/Pt plating. Hmmm.
Possibly, are you speaking of an alumina substrate having Ag/Pt
metallization (traces) on it?
Steve Creswick - Gentex
-----Original Message-----
From: Jose Antonio Garcia Ontalba [mailto:[log in to unmask]]
Sent: Wednesday, August 25, 2004 10:59 AM
To: [log in to unmask]
Subject: [TN] Corrosion in lead frames
Hello together!
I have an hybrid circuit with lead frames for bonding encapsulated with gel.
These lead frames are used for bonding the wires of aluminium only with heat
(without using solders, flux, etc.). We have made some durations test, after
them appears some red-orange spots on the lead frames preferably in the
borders, and, in some cases, comes into view blue parts too. We have seen
with Infra-Red photographs that this part (wire+lead frame) is by far the
warmest of the PCB when it is working, because through it comes high
electric flow.
The lead frames have a coating of Ag/Pt and the gel's major components are:
silicone, Pt (polymerization's activator) and alumina (for the thermal
conductivity). The lead frames have not solder nor flux residues.
So, anybody could tell me what is happening in the lead frame? I suppose
that a chemical reaction involves the Ag and/or the Pt but I have no idea
which could be!
Thank you all for your help!
Best regards
--
José Antonio García Ontalba
Quality department
NAGARES, S.A.
Ctra. Madrid-Valencia, Km. 196
16200 Motilla del Palancar (Spain)
Tel: 00 34 969 18 00 21
Fax: 00 34 969 33 11 31
E-mail: [log in to unmask]
--
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
-----------------------------------------------------
__________ Información emitida por NOD32 __________
Este mensaje ha sido verificado por NOD32 Antivirus System.
http://www.nod32.com
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
-----------------------------------------------------
__________ Información emitida por NOD32 __________
Este mensaje ha sido verificado por NOD32 Antivirus System.
http://www.nod32.com
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------
|