Be careful. Holding pot temperature close to the eutectic will result in
copper/tin dendrites forming at the bottom of the pot. These dendrites will
not melt at normal soldering temperatures only dissolve so there is a danger
of blocking ports preventing circulation and dissolution.
Always run the pump for some time to allow the copper tin crystals that
form during cooling to dissolve before processing boards.
-----Original Message-----
From: Colin McVean [mailto:[log in to unmask]]
Sent: Thursday, August 19, 2004 1:09 PM
To: [log in to unmask]
Subject: Re: [TN] Allowable copper contamination for SAC 305?
Either run two types of bar, or perform regular dragout of copper rich
dross, by running the pot cool for a period of time, and skimming the top
out. It's how we treat our HASL process.
Regards,
Colin McVean
Circuit Manufacture Ltd
Unit 9-12
Rowleys Green Lane
Longford
Coventry
CV6 6AG
Tel: 02476 666168
Fax: 02476 637089 ________________________________________________
This email is confidential and intended solely for the use
of the individual to whom it is addressed. Any views or opinions presented
are solely those of the author and do not necessarily represent those of the
Company.
If you are not the intended recipient, be advised that you
have received this email in error and that any use, dissemination,
forwarding, printing, or copying of this email is strictly prohibited.
If you have received this email in error please notify the Company by
telephone on +44 (0)24 7666 6168 or reply by email to the sender and delete
the email. ________________________________________________
Whilst every effort has been made to ensure that there are
no viruses embedded in this email, we highly recommend
that you virus scan any attached files using your own anti- virus software.
-----Original Message-----
From: TechNet [mailto:[log in to unmask]]On Behalf Of Dave Chapman
Sent: 19 August 2004 12:57
To: [log in to unmask]
Subject: Re: [TN] Allowable copper contamination for SAC 305?
We just returned from a seminar by Cookson which said 1% would be
contamination point. Additional solder bars without copper would need to be
added to bring the balance in line. I imagine now we would need to have SAC
bars and SA bars to keep balance, either way close monitoring of pot
composition seems to be inevitable. Dave C.
-----Original Message-----
From: Richard Kraszewski [mailto:[log in to unmask]]
Sent: Wednesday, August 18, 2004 4:08 PM
To: [log in to unmask]
Subject: [TN] Allowable copper contamination for SAC 305?
If one was to use a SAC305 alloy in a wave or selective soldering
application, how much copper contamination do you think would be allowable
before the melting range would become unacceptable. From what I can see from
the phase diagram, it appear one might be OK until you reached ~ 0.8-0.9%
copper?
Your thoughts would be appreciated.
Rich K / KEDS
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in the
BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in the
BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in the
BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet
NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send
e-mail to [log in to unmask]: SET Technet Digest Search the archives of
previous posts at: http://listserv.ipc.org/archives Please visit IPC web
site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
ext.5315
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------
|