I would not strip solder and re-level as any solder stripper would also
attack the copper. Our experience with stripping reflowed tin/lead has in
many cases reduced hole wall copper thickness below acceptable requirements.
Running the parts thru HAL once more is usually an acceptable rework for
this issue although I do not believe this is addressed in IPC specs.
James Hofer
Director of Operations
Accurate Circuit Engineering
3019 S. Kilson Dr.
Santa Ana Ca. 92707-4202
714-546-2162 work
714-473-6127 cell
[log in to unmask]
----- Original Message -----
From: "Eddie Rocha" <[log in to unmask]>
To: <[log in to unmask]>
Sent: Wednesday, August 25, 2004 9:06 AM
Subject: Re: [TN] Low solder rework
> Rework is due to solder thknss. I've re-HASL'd before with success but
with
> prototype orders. One of my concerns is: does IPC have a position on this
> type of rework?
>
> -----Original Message-----
> From: TechNet [mailto:[log in to unmask]]On Behalf Of Tom Gervascio
> Sent: Wednesday, August 25, 2004 5:22 AM
> To: [log in to unmask]
> Subject: Re: [TN] Low solder rework
>
>
> The question would be why are they being reworked? Is it solderability or
> solder thickness related?
>
> Re-HASL might grow a thicker layer of copper tin intermetallic. I would
> think removing the solder chemically, re cleaning and HASL would be
> desirable.
>
> My two cents worth
>
> >>> [log in to unmask] 08/24/04 06:14PM >>>
> Is there a rework spec or standard for bare PCB's with low solder? Would
it
> be acceptable to simply re-HASL (hot-air-solder-level)them? Any
reliablility
> issues with re-HASL? These are class 3 type bds.
> Thanks in advance for your help.
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 1.8e
> To unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt or (re-start) delivery of Technet send e-mail to
> [log in to unmask]: SET Technet NOMAIL or (MAIL)
> To receive ONE mailing per day of all the posts: send e-mail to
> [log in to unmask]: SET Technet Digest
> Search the archives of previous posts at: http://listserv.ipc.org/archives
> Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
> for additional information, or contact Keach Sasamori at [log in to unmask] or
> 847-509-9700 ext.5315
> -----------------------------------------------------
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 1.8e
> To unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt or (re-start) delivery of Technet send e-mail to
> [log in to unmask]: SET Technet NOMAIL or (MAIL)
> To receive ONE mailing per day of all the posts: send e-mail to
> [log in to unmask]: SET Technet Digest
> Search the archives of previous posts at: http://listserv.ipc.org/archives
> Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
> for additional information, or contact Keach Sasamori at [log in to unmask] or
> 847-509-9700 ext.5315
> -----------------------------------------------------
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 1.8e
> To unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
> To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
> Search the archives of previous posts at: http://listserv.ipc.org/archives
> Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
> -----------------------------------------------------
>
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------
|
|
|