7628 is the lowest resin content (%) prepreg generally available (which is
why it's cheaper), and filling 2 oz copper takes a lot of resin. 7628 is
about 40-44% RC, while 2113/2313/2116 are 54-56%, 1080 is 62-65% and 106 is
72-75%.
It's better to do something like:
-----2 oz Cu----
2113
7628
2113
-----2 oz Cu----
than:
-----2 oz Cu----
7628
7628
-----2 oz Cu----
Tim Reeves
-----Original Message-----
From: TechNet [mailto:[log in to unmask]]On Behalf Of Parial Swati
Sent: Thursday, July 15, 2004 8:41 PM
Subject: Re: 7628 prepreg?
Why is it that laminate voids are likely with such a combination ?
Regards,
Swati...
****************************************************************************
***
7628 aginst 2 oz copper is not recommended. Possible lamination issues are
likely, i.e. lam voids.
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------
|
|
|