TECHNET Archives

July 2004

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Content-Type:
text/plain; charset="iso-8859-1"
Sender:
Subject:
From:
"Dehoyos, Ramon" <[log in to unmask]>
Date:
Thu, 8 Jul 2004 05:31:40 -0700
MIME-Version:
1.0
X-To:
"TechNet E-Mail Forum." <[log in to unmask]>, [log in to unmask]
Reply-To:
"TechNet E-Mail Forum." <[log in to unmask]>, "Dehoyos, Ramon" <[log in to unmask]>
Parts/Attachments:
text/plain (76 lines)
        Hi Steve:
                        As everybody knows, solder balls are potentially a disaster if they ever get loose, unless they are CCed. For the time being, until a process is found to eliminate them, have you considered to have the adapters manually soldered?
                `       I agree with other comments, trapped air escaping too fast is causing solder to come up as droplets. Perhaps looking for  another adapter design.
        Regards,
        Ramon




-----Original Message-----
From: TechNet [mailto:[log in to unmask]]On Behalf Of Steve Gregory
Sent: Wednesday, July 07, 2004 6:44 PM
To: [log in to unmask]
Subject: Re: [TN] whatever happened


Hi Phil!

Well, as far as I know, it still is happening (I'm on vacation now in the
beautiful state of North Carolina at my parents home), but before I left, we
tried everything, and I do mean everything, trying to eliminate them, and nothing
worked. Here's what we tried:

1. Wave Solder Profile - Changed conveyer speeds, slowed it down, sped it up
all to no avail, still have the solderballs.

2. Preheat Settings - Increased preheat temperatures, decreased preheat
temperatures, nothing made a difference, still have the solderballs.

3. Stand-offs for the Adapter - Used dissolvable spacers to stand-off the
part, didn't help, still have the solderballs.

4. Pre-tinned the Adapter, didn't help, still have the solderballs.

5. Changed flux in the spray fluxer from OA to RMA, didn't help, still have
the solderballs.

6. Used Kyzen Aquanox 4512P and made a special recipe for these assemblies by
increasing the wash time to 20-minutes, didn't wash them away, still have the
solderballs.

The only way to remove them, is by brushing them away, and what gets me, is
that they brush away SO EASILY. They just won't wash off, and I can't keep them
from occuring where these Aries adapters are being used (6-per assembly).
There rest of the assembly looks great, and always has for the couple of years
we've been building it.

I'm just defeated for now, trying to figure out why these solderballs are
occuring. Hole diameter in the board is .040" and the lead diameter is around
.017" to .018".

-Steve Gregory-

> to your volcanic soldering process?


---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------

ATOM RSS1 RSS2