Looks like it should be easy. Could the solder pot not be level and you are running deeper immersion depths along he connector edge? Could you run a led check glass and see if there is flux on the pate before the chip wave and if the glass is clear after exiting the lambda/A nozzle? Maybe the flux is being burned off after the chip wave - are you running in air or nitrogen?
Tom Gervascio
Senior Process Engineer
Sparton Electronics
(352) 540-4040
>>> [log in to unmask] 07/23/04 01:46PM >>>
Below are the parameters that our wave operator reported.
Flux: No-clean Indium 3590-TX
The following are conveyor speeds and what they yield:
6.0 FPM yields a topside temperature of 206 Degrees F and a
solder dwell of 1.1 S. (via wave optimizer readings)
5.0 FPM yields a topside temperature of 223 Degrees F and a
solder dwell of 1.4 S. (via wave optimizer readings)
Preheat temps are 700 degrees F (zone 1) and 750 degrees F (zone 2)
Solder temp is 500 degrees F
I have used immersion depths of 0.032 and 0.024 for this assembly.
Rich
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Steve Gregory
Sent: Friday, July 23, 2004 9:16 AM
To: [log in to unmask]
Subject: Re: [TN] Solder Bridging on a Thru-hole connector
Hi Rich!
Finally got your picture, and it's posted. Go to:
http://www.stevezeva.homestead.com/files/Solder_Bridging.jpg
This picture is pretty blurry, but it's clear enough to see that you
shouldn't be having bridging problems with this connector. It's a
standard-pitch
dual-row connector, and there shouldn't be bridging problems with it.
Can you share with us the parameters for the wave that you're using?
Belt speed?
Pre-heat temperature?
Pot Temperature?
Flux Type?
I see from your web page that you have an Electrovert Econopak Plus 400
wave
machine, with a Sonotech spray fluxer. This machine should be capable of
waving that connector without bridges.
In the meantime, here's a link that has a pretty good troubleshooting
guide
for wave soldering defects. It's based on IPC-S-816. It's not the
end-all for
troubleshooting problems, but a good starting point.
http://www.ecd.com/retrieveFile.asp?file=WS_Expert_Guide.pdf
-Steve Gregory-
> Hello everyone,
>
> I am currently encountering a wave solder issue that I would like to
ask
> your opinion about. I have a dual row connector (Molex part #
> 70246-1621) that accumulates soldering bridging in a group of three.
I
> sent Steve an e-mail to see if he could post the picture on his
website
> so hopefully he can but until then I'll try and give you a generic
idea
> of how it is bridging. (The "arrow's" below represent the bridging
> between the leads) The wave operator has tried different speeds and
> board directions but continues to struggle with this particular
> connector.
>
> If anyone has any input I would appreciate it.
>
> TIA,
>
> Rich
>
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
ext.5315
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest