Have exactly same experience! Ray's pictures seem to picked from my own technical report years ago! Funny..
If the ceramic surface is impure + flux residues + little humidity + more than 5VDC..then these XMas trees will sometimes grow. Silver most commonly seen. We video recorded the thing...growth from one end to the other of the cap took less than one minute!
The cap manufacturer adjusted the improper end metallisation, we adjusted the flux, and the phenomenon is never seen any more.
Ingemar Hernefjord
Ericsson Microwave Systems
This communication is confidential and intended solely for the addressee(s). Any unauthorized review, use, disclosure or distribution is prohibited. If you believe this message has been sent to you in error, please notify the sender by replying to this transmission and delete the message without disclosing it. Thank you.
E-mail including attachments is susceptible to data corruption, interruption, unauthorized amendment, tampering and viruses, and we only send and receive e-mails on the basis that we are not liable for any such corruption, interception, amendment, tampering or viruses or any consequences thereof.
-----Original Message-----
From: TechNet [mailto:[log in to unmask]]On Behalf Of Steve Gregory
Sent: den 4 maj 2004 15:53
To: [log in to unmask]
Subject: Re: [TN] Crystalline growth across a capacitor...the next stage
Hi Ray!
I've posted your EDX up on my page too...
-Steve Gregory-
> Guys
>
> Great stuff! Did you find source?
>
> I’ve attached the EDX that was done on the area.
>
> Ray Alberty
>
> Quality Engineer
>
> Telematics and Homelink
>
> Jabil Circuit
>
> 3800 Giddings
>
> Auburn Hills, MI 48326
>
> Phone:248-292-6152
>
> Pager: 248-407-1909
>
> Fax: 248-292-6903
>
>
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------
|
|
|