HI SJ,
David asked you good questions.
Given your second e-mail, there are a number of possibilities:
(1) interfacial cracks developed during transport mechanical shock
loading--this would occur is
(a) not all solder balls were properly wetted--causes: insufficient
reflow temperature/ solderability
problems;
(b) weak interfacial attachment [prime suspect: ENIG-'black pad'].
(2) no wetting has taken place [component warpage, PWB warpage during reflow]
or insufficient solder paste.
In order to get a more succinct advice, you need to determine the actual
failure mode and failure root cause(s).
Regards,
Werner Engelmaier
Engelmaier Associates, L.C.
Electronic Packaging, Interconnection and Reliability Consulting
7 Jasmine Run
Ormond Beach, FL 32174 USA
Phone: 386-437-8747, Fax: 386-437-8737
E-mail: [log in to unmask], Website: www.engelmaier.com
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------
|
|
|