Hi Carrie:
One more thing to try. Spray the board with flux, heat up the flux with a heat gun, the white haze should disappear based on your soldering iron experience, then immerse it in alcohol and brush off the flux. It may also work without using heat.
Regards,
Ramon
> -----Original Message-----
> From: Brian Ellis [SMTP:[log in to unmask]]
> Sent: Saturday, April 24, 2004 8:04 AM
> To: [log in to unmask]
> Subject: Re: [TN] White Discoloration -- Excessive Heat, Insufficiently Cured SM, or, Both?
>
> WHOA!!!!!!!!!!!!!!!!!!!!!!!!!!!!
>
> IMPORTANT!
>
> Methyl chloroform is a popular but incorrect name for
> 1,1,1-trichloroethane (TCA), a relatively mild but unstable solvent and
> fairly useless for cure testing.
>
> Methylene chloride, aka dichloromethane (DCM), is a totally different
> beast and is more aggressive and better for cure testing.
>
> TCA is an ozone-depleting solvent and a controlled substance under the
> Montreal Protocol. As such, it has not been available in developed
> countries since 1 Jan 1996. Its instability gives it, assuming correct
> stabilisation, a useful lifetime of ~2 years. If your stuff was made
> before 1996, you can reckon it is useless, as a solvent, by now. In most
> countries, you are bound to have existing stocks and waste solvent
> destroyed by an approved destructor. You are probably not allowed to
> simply store it passively or to landfill it. Please check with your
> local authorities.
>
> Brian
>
> Morse, Carrie wrote:
> > Wow,
> > Thanks to everyone for all the info.
> > I have a new update. We tried 4 things based on a number of
> > recommendations:
> > 1. Applied flux and hit the area with an iron. The discoloration went
> > away. But, we have such a large area on so many boards there is no real
> > way to get this done in a timely fashion. In addition, we scratched the
> > area up pretty well, so, either way, it looks bad.
> > 2. We tried to re-wave the board. The discoloration got whiter/hazier
> > 3. Used Methyl Chloroform to test for permanency. No mask was evident
> > on the swab which tells me the mask is cured.
> > 4. Lastly, we baked a board at 250F for 45 minutes -- no change.
> >
> > So...Any ideas what it is or if it is detrimental?
> > Any suggestions?
> > It's Friday...If anyone can suggest the boards are OK and I can feel
> > comfortable to ship that would be fine by me.
> >
> > -Carrie
> >
> > -----Original Message-----
> > From: TechNet [mailto:[log in to unmask]] On Behalf Of Gregg Klawson
> > Sent: Friday, April 23, 2004 11:50 AM
> > To: [log in to unmask]
> > Subject: Re: [TN] White Discoloration -- Excessive Heat, Insufficiently
> > Cured SM, or, Both?
> >
> > Carrie,
> >
> > Some info from one SM mfr, this may help.
> >
> > http://www.enthone.com/electronics/pdf/Imup5.pdf
> >
> > -- Gregg
> >
> > At 02:27 PM 4/22/2004, Morse, Carrie wrote:
> >
> >>Here's the status. I baked the boards for 45min @ 250F and...I still
> >>have the white haze. No change. So, What do you all think?
> >>(IOW--HELP!!!!)
> >>
> >>-Carrie
> >>
> >>-----Original Message-----
> >>From: Brian Ellis [mailto:[log in to unmask]]
> >>Sent: Thursday, April 22, 2004 2:06 AM
> >>To: TechNet E-Mail Forum.; Morse, Carrie
> >>Subject: Re: [TN] White Discoloration -- Excessive Heat, Insufficiently
> >
> >
> >>Cured SM, or, Both?
> >>
> >>I'm not saying that this is the cause, but another possibility is
> >>hydrolysis of the uncured solder mask. If the boards are coated and
> >>then stored in a humid atmosphere before development (either before or
> >>after
> >>exposure) for more than an hour or two, then some components in the
> >>chemistry may absorb sufficient humidity to hydrolyse, partially
> >>upsetting the polymerisation.
> >>
> >>I suggest methylene chloride would be better than acetone for a wipe
> >>test, but it depends on the chemistry of the LPI.
> >>
> >>Brian
> >>
> >>Morse, Carrie wrote:>
> >>
> >>>We are wave soldering a LPI board and seeing a Whitish Discoloration
> >>>-- Haze like -- only in the areas that the board has seen OA flux
> >>>and
> >>
> >>wave.
> >>
> >>>We are using a wave pallet and the areas not exposed do not exhibit
> >>>this phenomena. This board is also processed through SMT for one
> >>>side
> >>
> >>>and we do not see this around any of the SMT.
> >>>
> >>>We have not seen this problem in the past, and, the Wave operator
> >>>states that the wave recipe has not changed.
> >>>
> >>>So, I am wondering -- if LPI is not fully cured, will it turn white
> >>>when exposed to OA flux and Wave?
> >>>Also, what IS the max temp LPI should be able to see and for how
> >>>long without discoloring?
> >>>We've done an Acetone test, but, it comes up clean and....I think I
> >>>read in a previous posting that the Acetone may not be an effective
> >>>test for LPI. Is that true? If so, What IS an effective test?
> >>>
> >>>I'm headed to the Omega tester to see "how clean" the board is.
> >>>
> >>>All advice is welcome!
> >>>
> >>>-Carrie
> >>>
> >
> >
> > ---------------------------------------------------
> > Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
> > unsubscribe, send a message to [log in to unmask] with following text in
> > the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
> > (re-start) delivery of Technet send e-mail to [log in to unmask]: SET
> > Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
> > posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
> > archives of previous posts at: http://listserv.ipc.org/archives Please
> > visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
> > additional information, or contact Keach Sasamori at [log in to unmask] or
> > 847-509-9700 ext.5315
> > -----------------------------------------------------
> >
> > ---------------------------------------------------
> > Technet Mail List provided as a service by IPC using LISTSERV 1.8e
> > To unsubscribe, send a message to [log in to unmask] with following text in
> > the BODY (NOT the subject field): SIGNOFF Technet
> > To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
> > To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
> > Search the archives of previous posts at: http://listserv.ipc.org/archives
> > Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
> > -----------------------------------------------------
> >
> >
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 1.8e
> To unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
> To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
> Search the archives of previous posts at: http://listserv.ipc.org/archives
> Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
> -----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------
|