I'm not saying that this is the cause, but another possibility is
hydrolysis of the uncured solder mask. If the boards are coated and then
stored in a humid atmosphere before development (either before or after
exposure) for more than an hour or two, then some components in the
chemistry may absorb sufficient humidity to hydrolyse, partially
upsetting the polymerisation.
I suggest methylene chloride would be better than acetone for a wipe
test, but it depends on the chemistry of the LPI.
Brian
Morse, Carrie wrote:
> We are wave soldering a LPI board and seeing a Whitish Discoloration --
> Haze like -- only in the areas that the board has seen OA flux and wave.
> We are using a wave pallet and the areas not exposed do not exhibit this
> phenomena. This board is also processed through SMT for one side and we
> do not see this around any of the SMT.
>
> We have not seen this problem in the past, and, the Wave operator states
> that the wave recipe has not changed.
>
> So, I am wondering -- if LPI is not fully cured, will it turn white when
> exposed to OA flux and Wave?
> Also, what IS the max temp LPI should be able to see and for how long
> without discoloring?
> We've done an Acetone test, but, it comes up clean and....I think I read
> in a previous posting that the Acetone may not be an effective test for
> LPI. Is that true? If so, What IS an effective test?
>
> I'm headed to the Omega tester to see "how clean" the board is.
>
> All advice is welcome!
>
> -Carrie
>
>
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 1.8e
> To unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
> To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
> Search the archives of previous posts at: http://listserv.ipc.org/archives
> Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
> -----------------------------------------------------
>
>
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------
|
|
|