As co-chairman of the 4-14 plating committee that is responsible for surface
finish specifications I must take issue with the comments from Mr. Bush.
There is no doubt that ENIG is a complicated process that requires
monitoring and proper process control, the 4552 document clearly indicates
that not following proper procedures, use of automated dosing systems and
adherence to chemical suppliers instructions will lead to problems. In fact
it was one of my personal goals for this specification to help identify the
Enig suppliers who believe it is too troublesome a process to run correctly
and stop the OEM's / CM's from buying sub standard product which has
unfortunately given ENIG such a bad reputation.
Both immersion silver and immersion tin are not without their issues either.
Similar process control needs to be demonstrated for these chemistries as
well, purchasing either finish from a supplier with a laissez-faire attitude
towards control and more importantly an emphasis on cost over product
quality is a recipe for disaster.
Regards
Gerard O'Brien
Co-chairman 4-14 plating committee
Photocircuits Corporation.
-----Original Message-----
From: Jeffrey Bush [mailto:[log in to unmask]]
Sent: Monday, March 29, 2004 8:15 AM
To: [log in to unmask]
Subject: Re: [TN] Black Pad Prevalence
ENIG processes are costly to maintain and this finish if not the
preferred solution for soldering planarity. The Nickel deposition
process requires a good deal of attention and the main issue is the
process going south is the lack of work being processed through it. The
cost of ownership of the ENIG outweighs the benefits sharply and both
tin and silver exist as economic alternatives to gold and do not have
the disadvantages which go beyond the black pad condition. Silver
appears to be the most effective alternative as it is more forgiving for
time delays between thermal excursions, but many assemblers have adapted
their process to also run tin effectively, which has the lowest overall
cost impact per unit.
Stay away from ENIG and evaluate tin and/or silver.
Jeffrey Bush
Director, Quality Assurance and Technical Support
76 Technology Drive - POB 1890
Brattleboro, Vermont 05302-1890
Tel. 802.257.4571.21 Fax. 802.257.0011
[log in to unmask]
http://www.vtcircuits.com
-----Original Message-----
From: Paul Truit [mailto:[log in to unmask]]
Sent: Saturday, March 27, 2004 10:03 AM
To: [log in to unmask]
Subject: [TN] Black Pad Prevalence
I have searched the archives and have found lot's of good info but
nothing in regard to the prevalence or the statistical occurrences of
this event.
I have run tens of thousands of ENIG boards and I haven't observed this
defect but I am concerned enough to ask. Is this a board fabricator
controllable issue that has been minimized?
Have you observed this phenomenon? How often will this occur? Is
immersion silver the better way to go to assure the reliability and
quality of the products?
--
Paul Truit, Mfg. Eng.
RBB Systems, Inc.
4265C E. Lincolnway
Wooster, OH 44691
Ph. (330) 567-2906 ext 514
Fax (330) 263-5324
Email: [log in to unmask]
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
archives of previous posts at: http://listserv.ipc.org/archives Please
visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------
|