Back in the mid-90's while at Motorola, we conducted a cursory evaluation of
PbSn flip chip assembly using square pads vs. round and contrary to initial
expectation, the square pads showed greater temp cycles to failure. Without
a large amount of study this appeared to be the consequence of the large
contact interface area with a square of dimension 'x', vs a round pad with
diameter 'x'. This may or may not be relevant to the PbFree discussion.
Regards,
Leo
------------------------------------
Leo M. Higgins III, Ph.D.
ASAT Inc.
Central Region Mgr. / Director of Sales
[log in to unmask]
3755 Capital of Texas Hwy-So
Suite 100
Austin, TX USA 78726
tel: 512-383-4593
fax: 512-383-1590
mobile: 512-423-2002
------------------------------------
-----Original Message-----
From: Brian J. Toleno, Ph.D. [mailto:[log in to unmask]]
Sent: Wednesday, March 24, 2004 1:12 PM
To: [log in to unmask]
Subject: Re: [TN] FW: Round SMT pads
It is not an issue of reliability (to my knowledge that hasn't been
tested, but I don't see how it would be a major impact as long as you have
good fillets on the leads). This is more of an appearance issue. This
is especially true with OSP pads where the exposed copper may eventually
green.
Brian J. Toleno, Ph.D.
Sr. Applications Chemist
Loctite Electronics
15051 East Don Julian Rd
Industry, CA 91746
Ph: 626-968-6511 x304
Cell: 626-215-0879
**********************************************************************
This email and any files transmitted with it are confidential and
intended solely for the use of the individual or entity to whom they
are addressed. If you have received this email in error please notify
the system manager.
This footnote also confirms that this email message has been swept by
MIMEsweeper for the presence of computer viruses.
http://www.loctite.com/
**********************************************************************
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------
|
|
|