This 35ppm that DuPont gives is an average: 27ppm below Tg, 45 above. Therefore lower expansion than the FR4.
Tony Steinke <[log in to unmask]> wrote:
Frank,
After reviewing my data sheets for the CB100 theTg
of the cured silver epoxy is only 115C with a 35ppm TCE, I imagine that
would explain what you experienced on your boards. The key word is
"Conductive ViaPlug" not "Conductive ThruHole Plug"
Tony Steinke
AIT-Atlanta Inc.
Tony Steinke
----- Original Message -----
From: "Franklin Asbell"
To:
Sent: Tuesday, March 23, 2004 1:08 PM
Subject: Re: [TN] PWB delamination and silver epoxy fill
> The reason I say they are probably large vias is we had seen that once in
> the past. Customer spec'd a 28 mil via with silver epoxy fill. They placed
a
> heavy BGA component right over those filled 28 mil pads/vias...the larged,
> silver-filled vias acted as a heat-sink drawing too much heat into them
> causing delamination only around those vias. We reduced the hole size, the
> problem went away. We also did another job for them where we could not
> reduce the hole size, we used ceramic fill instead of epoxy, no problems
at
> all... Just one persons experience, hope this helps...
>
> Franklin
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 1.8e
> To unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
> To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
> Search the archives of previous posts at: http://listserv.ipc.org/archives
> Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
> -----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------
Do you Yahoo!?
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------
Yahoo! Finance Tax Center - File online. File on time.
|
|
|