The issue being encountered is a likely due to an under-cut of the
soldermask during the white tin application process. White tin requires a
microecth of the copper surface prior to exchange of the tin to the board
surface. This microetch, and certainly a re-processing of boards typcial
to white tin finishing, begins to affect the bond of the soldermask to the
copper along the permeter of the land areas. The smaller the perimeter
area, like a trace into the fine pitch device, has a propensity for
increased etching from the energy created from the chemistry.
This condition will be typical in a IT, IS and ENIG finishes. Genrally IT
and IS can be re-processed for issues from storage and this amplifies the
condition. Be sure that your pre-heat and reflow temperatures are not
increased to high for the lead-free soldering - IT should process similar
to solder if shelf-life, storage and handling practices are controlled well.
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------
|
|
|