TECHNET Archives

February 2004

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
"TechNet E-Mail Forum." <[log in to unmask]>, David Douthit <[log in to unmask]>
Date:
Fri, 13 Feb 2004 17:52:37 -0500
Reply-To:
"TechNet E-Mail Forum." <[log in to unmask]>, - Bogert <[log in to unmask]>
Subject:
MIME-Version:
1.0
Content-Transfer-Encoding:
quoted-printable
Content-Type:
text/plain; charset="iso-8859-1"
From:
- Bogert <[log in to unmask]>
Parts/Attachments:
text/plain (86 lines)
February 13, 2004

I have no info on solder joint reliability when using pure tin.  However, we had an application where we had a metal box holding several high precision resistors used in a circuit with very low current.  The box was plated with pure tin.  We saw numerous tin whiskers growing at right angles to the sides of the box.  However, since they were very small in length, they did not cause any problems. Normally, even if the whiskers short to an adjacent conductor, they will quickly burn open.  We cleaned off the whiskers then coated the box sides with conformal coating which prevented subsequent whiskers/
  ----- Original Message ----- 
  From: David Douthit<mailto:[log in to unmask]> 
  To: [log in to unmask]<mailto:[log in to unmask]> 
  Sent: Friday, February 13, 2004 12:08 PM
  Subject: Re: [TN] Pure Tin Component Finish


  Scott,

  Go to: http://www.nepp.nasa.gov/whisker/index.html<http://www.nepp.nasa.gov/whisker/index.html>
  For the latest and greatest on tin whiskers.

  David A. Douthit
  Manager
  LoCan LLC

  Newland, Scott wrote:

  >During our resent lead free evaluation it was discovered that several of our
  >component vendors are changing their finishes from tin- lead to pure tin.  Quite
  >often this change is being made with no part number change, so these part are
  >getting to our manufacturing floor without anyone knowing they have a different
  >finish.  This has lots of people's attention due to the Hi Rel nature of most of
  >our products.  We have narrowed our concerns to two:  tin whiskers and solder
  >joint reliability.  There is a lot of work being performed on tin whiskers.  Do
  >you see the pure tin component finish impacting the tin- lead solder joint
  >metallurgy to the point of impacting high or low cycle fatigue??  Typical I
  >would think the component finish would be a small percentage of the total volume
  >of the solder joint, resulting in minimal impact.  But I'm afraid the
  >inter-metallic layers maybe impacted, resulting in changed reliability.
  >
  >The opinions of this group would be valued.
  >
  >
  >Scott Newland
  >Harris GSCD
  >321 727 6472
  >Pager  321 690 4131
  >E-Mail  <mailto:[log in to unmask]<mailto:[log in to unmask]>> [log in to unmask]<mailto:[log in to unmask]>
  >For a brain teaser try:
  > <http://pao.gsfc.nasa.gov/science.html<http://pao.gsfc.nasa.gov/science.html>> http://pao.gsfc.nasa.gov/science.html<http://pao.gsfc.nasa.gov/science.html>
  >
  >This information is only intended for the use of the individual or entity named
  >in this email.  If you are not the intended recipient, you are hereby notified
  >that any disclosure, copying, distribution, or use of the contents of this
  >information is strictly prohibited.  If you have received this email in error,
  >please notify me and delete it immediately.
  >
  >
  >---------------------------------------------------
  >Technet Mail List provided as a service by IPC using LISTSERV 1.8e
  >To unsubscribe, send a message to [log in to unmask]<mailto:[log in to unmask]> with following text in
  >the BODY (NOT the subject field): SIGNOFF Technet
  >To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]<mailto:[log in to unmask]>: SET Technet NOMAIL or (MAIL)
  >To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]<mailto:[log in to unmask]>: SET Technet Digest
  >Search the archives of previous posts at: http://listserv.ipc.org/archives<http://listserv.ipc.org/archives>
  >Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16<http://www.ipc.org/contentpage.asp?Pageid=4.3.16> for additional information, or contact Keach Sasamori at [log in to unmask]<mailto:[log in to unmask]> or 847-509-9700 ext.5315
  >-----------------------------------------------------
  >
  >
  >
  >

  ---------------------------------------------------
  Technet Mail List provided as a service by IPC using LISTSERV 1.8e
  To unsubscribe, send a message to [log in to unmask]<mailto:[log in to unmask]> with following text in
  the BODY (NOT the subject field): SIGNOFF Technet
  To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]<mailto:[log in to unmask]>: SET Technet NOMAIL or (MAIL)
  To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]<mailto:[log in to unmask]>: SET Technet Digest
  Search the archives of previous posts at: http://listserv.ipc.org/archives<http://listserv.ipc.org/archives>
  Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16<http://www.ipc.org/contentpage.asp?Pageid=4.3.16> for additional information, or contact Keach Sasamori at [log in to unmask]<mailto:[log in to unmask]> or 847-509-9700 ext.5315
  -----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------

ATOM RSS1 RSS2