the G-12 committee as well as the NASA whisker site simply suggests the
following:
a. there is no single event that promotes Sn whiskers
b. for every theory like this, there is enough contradicting evidence to
suggest other wise
c, it is all a matter of "reducing" the risk not eliminating it: in other
words if you mean" controlling it" as in "minimizing risk" then u are on
the right track.
Prasad Godavarti (Dr. G)
Guenter Grossmann
<Guenter.Grossman
[log in to unmask]> To
Sent by: TechNet [log in to unmask]
<[log in to unmask]> cc
Subject
01/26/2004 09:38 Re: [TN] Antw: [TN] Lead-free
AM Component Finishes
Please respond to
"TechNet E-Mail
Forum."
<[log in to unmask]>
; Please respond
to
Guenter Grossmann
<Guenter.Grossman
[log in to unmask]>
Jim
I was talking last week with a person from Motorola Germany and a
someone from Collini. In the discussion both told me that by using a Ni-
underplate and with the appropriate plating chemistry they don't' see
problems with whiskers anymore. Earlier, in a conference from
Electrosuisse, I had a discussion with a speaker talking about whisker
growth as a function of grain size of the Sn plating which can be
controlled with the appropriate chemistry and process parameters. What I
learned in these discussion was that whiskers are a problem that can be
controlled. In the worst case, in my understanding, it's a question of
money. Annealing the plating can reduce the internal stress in the
plating and diminish whisker growth.
Wrong?
Best regards
Guenter
EMPA
Swiss Federal Laboratories for Materials Testing and Research
Centre for Reliability
Guenter Grossmann, Senior Engineer
8600 Duebendorf
Switzerland
Phone: xx41 1 823 4279
Fax : xx41 1 823 4054
mail: [log in to unmask]
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------
|
|
|