Hi Phil! You have two phenomena to be concern with: oxidation of the
surface and intermetallic consumption of the solderable finish. The
intermetallic consumption issue is pretty simple - stay away from elevated
temperature storage (like 50C) and keep the solderable finish reasonable
thick. Oxidation tends to be the overwhelming issue. Moisture will cause
the oxidation reactions to be more degrading so avoiding moisture is a good
idea. Again, keeping the solderable coating thick (per the vendor's
recommendation) and keeping oxygen away from the finish will help reduce
degradation. No matter how good of nitrogen environment or amount of
moisture permeable bagging will eliminate the oxidation reactions but you
can minimize it to the best of your ability to delay the inevitable. Sorry
but nothing lasts forever! Good luck.
Dave Hillman
Rockwell Collins
[log in to unmask]
Phil Bavaro
<pbavaro@QUALCOMM To: [log in to unmask]
.COM> cc:
Sent by: TechNet Subject: [TN] Long term Solderability Preservation Methods
<[log in to unmask]>
12/11/2003 08:11
PM
Please respond to
"TechNet E-Mail
Forum."; Please
respond to Phil
Bavaro
Does anyone have any good suggestions for storage methods when business
reasons require an end of life buy of a PLCC which has a tin lead coating
on it and the quantity will last for the next six years of production?
Obviously these need to be kept as dry as possible, in an environmentally
controlled, esd protective dark/cool location, but the practical storage
issue of what container to place these in (several pallets
worth), strategic separation (in case of a fire or other disaster) and
security are also at hand.
I am not sure what the shelf life is for the best moisture vapor barrier
bags but I am thinking of double bagging the parts so that we can get rid
of the card board boxes they are in.
I am considering storage at cooler temperatures to slow down the oxidation
rate, but what about "nitrogen" purging before pulling the vacuum on the
parts. Will either of these methods make a difference?
It has been a while since I have worked on a program which kept stock for
anything longer than two months.
We brainstormed some pretty wild approaches to this today so I know that my
management is pretty open to anything still at this point.
Obviously lead free will not be a factor for this product until our
stockpile is depleted.
Thanks in advance.
Phil
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------
|
|
|