TECHNET Archives

December 2003

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
"TechNet E-Mail Forum." <[log in to unmask]>, Sasha Miladinovic <[log in to unmask]>
Date:
Thu, 4 Dec 2003 11:12:15 -0800
Reply-To:
"TechNet E-Mail Forum." <[log in to unmask]>, Ed Popielarski <[log in to unmask]>
Subject:
MIME-Version:
1.0
Content-Transfer-Encoding:
quoted-printable
Content-Type:
text/plain; charset="iso-8859-1"
From:
Ed Popielarski <[log in to unmask]>
Parts/Attachments:
text/plain (121 lines)
Sasha,

As stated by an earlier contributor, the tin rises to the top (more or less) and this is where the operators remove the dross along with solder. Just my guess, not fact. The tin drop is empirical observation over many (20+) years of being intimate with wave soldering. Always, when an analysis came back "off eutectic" tin was added. 100%, never saw one go the other way!

Have a safe and happy holiday!

Regards,

Ed Popielarski
QTA Machine
27291 Jardines
Mission Viejo, Ca. 92692

Phone:949-581-6601
Fax: 949-581-2448
Cel: 949-337-2578

WWW.QTA.NET

"Thank God for America...
before it's too late!"
  ----- Original Message ----- 
  From: Sasha Miladinovic 
  To: TechNet E-Mail Forum. ; Ed Popielarski 
  Sent: Thursday, December 04, 2003 10:17 AM
  Subject: Re: [TN] SnPb Solder pot composition



  Ed, 

  I like Your declaration about "cold" joints... :) I had a minor war i a earlier life with a Q-department about the definition.. :) 

  I'm not sure it any of us is right or wrong, but why would be Tin that drops? 
  Isn't it density and temparature that is the governing factors in this case? 

  Enyone outthere that can explain this? :) 

  *************************************************************************
  Sasha Miladinovic - Production Engineering 
  Amersham Biosciences, PCB Production, Umeå
  Tel:      +46 (0) 90 150 232
  Fax:     +46 (0) 90 138 372
  E-mail: [log in to unmask]
  *************************************************************************



       Ed Popielarski <[log in to unmask]> 
        Sent by: TechNet <[log in to unmask]> 
        2003-12-04 18:40 
        Please respond to "TechNet E-Mail Forum."; Please respond to Ed Popielarski 

               
                To:        [log in to unmask] 
                cc:         
                Subject:        Re: [TN] SnPb Solder pot composition 



  Yordan,

  Deviation from 63/37 can cause increased solder shorts in a wave soldering
  machine. At 63/37 (eutectic) the melt point is minimum, and there is no
  plasticus range. As you drift from there the melt point increases and the
  plastic range increases. This is why hand solder is preferred at 60/40...
  there IS plastic range and makes it easier to judge the joint as you solder.
  This is also the main cause of "frosty" joints (I hate to say "cold" since
  it is a very inaccurate term).

  Another thought to add to the mix is the accuracy of the lab. I recommend
  using either Alpha Metals or Kester to do the analysis (Type C which is the
  "whole enchilada" variety) and perhaps to rule out other variables discussed
  in other's postings, take a few samples, from the static part of the pot,
  from the wave after running at temperature, etc. If all the samples come
  back relatively the same, then you are good to go, but if one or two stand
  out, there could be something worth looking into.

  Additionally, (yes, another variable) the tin  is usually the element that
  drops, not the lead. This has me wondering as well. Why?

  Have a safe and happy holiday!

  Regards,

  Ed Popielarski
  QTA Machine
  27291 Jardines
  Mission Viejo, Ca. 92692

  Phone:949-581-6601
  Fax: 949-581-2448
  Cel: 949-337-2578

  WWW.QTA.NET

  "Thank God for America...
  before it's too late!"

  ---------------------------------------------------
  Technet Mail List provided as a service by IPC using LISTSERV 1.8e
  To unsubscribe, send a message to [log in to unmask] with following text in
  the BODY (NOT the subject field): SIGNOFF Technet
  To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
  To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
  Search the archives of previous posts at: http://listserv.ipc.org/archives
  Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
  -----------------------------------------------------



---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------

ATOM RSS1 RSS2