Ashok: Clear conversion coatings(probably chromate)are very thin and have
limited protective properties for the base metal. When subjected to heat
from the wash process in combination with caustic or high pH conditions from
the saponifier they can be easily stripped. Once stripped the base aluminum
metal continues to react with the caustic saponifier. Depending on the type
of aluminum alloy a black smut will form when exposed to caustic chemistry.
This is what I believe you are seeing.
I don't know what saponifier you are using but you may want to try it in a
lower concentration and/or lower wash temps. You may also want to explore a
more buffered saponifier that operates at a lower pH.
Regards
Michael Barmuta
Staff Engineer
Fluke Corp.
Everett WA
425-446-6076
-----Original Message-----
From: Dhawan, Ashok [mailto:[log in to unmask]]
Sent: Wednesday, December 17, 2003 1:12 PM
To: [log in to unmask]
Subject: [TN] Tarnished Surface
Technetters
Anyone who has experienced and resolved tarnishing of Aluminium surface upon
cleaning with DI water + saponifier. The aluminium surface is protected with
conversion coating (clear) which is turning black when exposed to saponifier
solution.
Ashok Dhawan P.Eng
Manufacturing Engineer
Solectron
Snailmail:1455 Mountain Avenue
Winnipeg MB R2X 2Y9 CANADA
* E-mail: [log in to unmask]
* Phone: (204) 631-7208
* Fax: (204) 631-7294
* I-net: <http://www.solectron.com>
Confidentiality Notice: This e-mail message, including any
attachments, is for the sole use of the intended recipient(s) and may
contain confidential and privileged information. Any unauthorized; review,
use, disclosure or distribution is prohibited. If you are not the intended
recipient, please contact the sender by reply e-mail and destroy all copies
of the original message.
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------
|
|
|