TECHNET Archives

December 2003

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
Date:
Mon, 15 Dec 2003 09:03:25 -0800
Reply-To:
David Hoover <[log in to unmask]>
Subject:
MIME-Version:
1.0
Content-Transfer-Encoding:
7bit
Content-Type:
text/plain; charset="iso-8859-1"
From:
David Hoover <[log in to unmask]>
Parts/Attachments:
text/plain (247 lines)
Steve,

It looks like the folks have really covered the potential Nickel oxidation
from the inside-out. I ran into this once before. I was thinking since the
package goes through two lamination processes you might want to
consider the lamination release sheets. They do a great job releasing
and usually release something on the surfaces too. If you do a surface
analysis you could find Silicones or Flourines that were (are) part of
your release sheet. An semi-aggressive plasma could clean some of
that off. Try to use a release sheet that has a very high thermal
resistance temperature (like skived PTFE). That tends not to
leave anything behind at the lam temperatures you mentioned.

Cheers,

Dave Hoover  (aka, Groovy)
----- Original Message -----
From: "Steve Kelly" <[log in to unmask]>
To: <[log in to unmask]>
Sent: Friday, December 12, 2003 10:32 AM
Subject: Re: [TN] Cleaning of Wire Bondable Gold


More Information:

The press cycles are a controlled ramp from room temperature to 340F over
approx. 45 minutes, cure for 70 minutes, controlled ramp down to room over
approx. 35 minutes. Pressure approx. 50 psi.
If it was nickel diffusion would that be approx. even across all pads or can
it be highly variable- most pads bond - the customer is only having issues
with a few (120 pads in the row - 8 mil pitch)



Regards Steve Kelly

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Leo Higgins
Sent: Friday, December 12, 2003 1:11 PM
To: [log in to unmask]
Subject: Re: [TN] Cleaning of Wire Bondable Gold

Hello all,
    Ni movement through Au porosity generally starts as Ni(OH)2, and no
diffusion through bulk or Au grain boundaries is involved.  The hydroxide is
black in appearance.  With adequate humidity, the hydroxide will 'grow' out
over the Au surface surrounding the void in the Au that exposed the
underlying Ni.  Over time/temperature the oxide will form from the
hydroxide.  Ni diffusion through Au thin films does not occur at high rates
until well over the 230-235C reflow temp noted below, and Ni diffusion
through Au (along GBs as noted below) would not be occuring at any
measurable rate at the rigid/flex lamination temperatures associated with
the question that initiated this string, but the hydroxide/oxide could be
forming in Au pores that exposed Ni.  The diffusion of Ni through Au was
studied heavily in the mid to late 80s when hermetic sealing of ceramic
packages with kovar lids was very common, and Au-Sn eutectic material was
used.  This eutectic melts at 280C and it is in the approximate 270 - 300C
range where Ni diffuses very rapidly through void-free Au.  Below 250C it
should not be an issue unless soak time is very long.

Best regards,
Leo

-----Original Message-----
From: Vladimir Igoshev [mailto:[log in to unmask]]
Sent: Friday, December 12, 2003 11:18 AM
To: [log in to unmask]
Subject: Re: [TN] Cleaning of Wire Bondable Gold


Hi Steve,

What kind of "surface nickel/diffusion"  data are you looking for? I'm a
little bit "confused" with diffusion "accelerated" (or promoted) by possible
voiding in the gold layer. I think the temperature isn't high enough to have
something like surface self-diffusion so, it doesn't look like the presence
of pores should affect possible diffusion of Ni through the Au layer.  I
agree with Joe, that some organic layer may be present on the surface and
could cause the problem (let say "develops" over time/temperature exposure).


Vladimir Igoshev
Research in Motion
(519)888-7465, x5283

-----Original Message-----
From: Steve Kelly [mailto:[log in to unmask]]
Sent: December 12, 2003 11:24 AM
To: [log in to unmask]
Subject: Re: [TN] Cleaning of Wire Bondable Gold


Hi Joe,

I have some answers:
1) soldering is normal no-clean - not lead free . We normally re-flow at
230-235 C (sees this temperature for approx. 40-45 seconds)
2) I am in the process of looking for surface nickel/diffusion. Will know
later today
3) the components are at one end of the flex - wire bond pads are about 4.5
inches away.
4) I am receiving a lot of opinions about how much gold should be there but
in general people are leaning to more - how much more is a good question
5) we also build another part for this same customer that only sees one
press cycle after gold and no re-flow - construction is a little different
(but gold/nickel/copper is on top of an AP in both cases). To the best of my
knowledge they have no issues with this part for over 4 years.

Regards Steve Kelly

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Joe Fjelstad
Sent: Friday, December 12, 2003 11:07 AM
To: [log in to unmask]
Subject: Re: [TN] Cleaning of Wire Bondable Gold

Hi Steve,

Interesting discussion you have brought to the fore and you have gotten some
excellent advice on cleaning. It was not stated but I am assuming gold wire
bonding based on the thickness and as well assuming that the gold is not
selectively plated on the wire bonding pads.

My experience from past lives was that 1 micron was normally enough,
however,
there were not two extra press cycles (with attendant volatilization and
deposition of organic materials and a reflow operation that preceded wire
bonding).

I have worked with folks wherein millions of devices were wire bonded post
reflow assembly using aluminum wedge bonding. The gold for such was about
1/5
micron

Brian has suggested and it has been seconded that porosity might be in the
mix.

I am left with a few questions whose answers that might lead me to ask
better
questions.

Is the soldering leadfree? (higher temperatures? volatilized organics? )

Have you looked at the positity/diffusion issue? (i.e. Is Ni really there?)

Or is the offending layer organic by analysis?

Last (for the moment anyway... ;-) what thickness of gold would be
considered
pore free? 1.5 microns?,  2.0?  2.1?  (I know that there are plating related
issues that mitigate any answer) and would that work for all steps in the
process? (embrittlement has already been cited as a concern but where is the
wall
for this process combination?)

Gold is expensive but not so expensive as the board. I have had customers in
the past that specified 1.5 microns and never had a problem (make that never
reported back a problem)

We all like a good problem but the real objective is to find a way to make
them never show their faces in production. It's pretty boring but very cost
effective :-)

Good luck,
Joe


---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------

ATOM RSS1 RSS2