TECHNET Archives

October 2003

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
Date:
Wed, 15 Oct 2003 18:38:16 -0500
Reply-To:
"TechNet E-Mail Forum." <[log in to unmask]>, [log in to unmask]
Content-type:
text/plain; charset=iso-8859-1
Subject:
From:
Dave Hillman <[log in to unmask]>
X-cc:
Content-transfer-encoding:
quoted-printable
MIME-Version:
1.0
Parts/Attachments:
text/plain (311 lines)
Hi folks! Thanks Bev but the silver tarnish data presented at the IPC Fall
meeting is Lenora Toscano's work (great stuff - great data - but not my
work!). The paper I presented dealt with overall general and galvanic type
corrosion impacts of the ENIG finish. Lenora presented solderability
performance results correlated to the amount of silver tarnish thickness -
very applicable data for assessing manufacturing issues.  There are a
number of companies in the industry who are making a risk assessment
evaluations of the potential of having a black pad issue versus the
positive attributes of the ENIG finish. It should be interesting to see the
direction folks go.

Dave


                                                                                                                                       
                      Bev Christian                                                                                                    
                      <[log in to unmask]        To:       [log in to unmask]                                                               
                      ET>                      cc:                                                                                     
                      Sent by: TechNet         Subject:  Re: [TN] ENIG solder joint embrittlement                                      
                      <[log in to unmask]>                                                                                                
                                                                                                                                       
                                                                                                                                       
                      10/15/2003 06:52                                                                                                 
                      AM                                                                                                               
                      Please respond to                                                                                                
                      "TechNet E-Mail                                                                                                  
                      Forum."; Please                                                                                                  
                      respond to Bev                                                                                                   
                      Christian                                                                                                        
                                                                                                                                       
                                                                                                                                       




Jim,
There was a paper by Toscano & Hillman (Rockwell) at the IPC Fall meeting
that shows that even when it looks bad it performs well. They treated it
with 85C/85%RH, salt fog or mixed flowing gas when in contact with Al, but
it did not corrode, passed electrochemical migration AND had suitable
contact resistance.
regards,
Bev Christian
Research in Motion

-----Original Message-----
From: Marsico, James [mailto:[log in to unmask]]
Sent: October 15, 2003 7:50 AM
To: [log in to unmask]
Subject: Re: [TN] ENIG solder joint embrittlement


Not having any experience with immersion silver on PWBs, I have a question.
In the past, silver plating was a problem because of tarnishing.  Was this
resolved?  How?

Jim Marsico
Senior Engineer
Production Engineering
EDO Electronics Systems Group
[log in to unmask] <mailto:[log in to unmask]>
631-595-5879


        -----Original Message-----
        From:   Wenger, George M. [SMTP:[log in to unmask]]
        Sent:   Tuesday, October 14, 2003 7:57 AM
        To:     [log in to unmask]
        Subject:        Re: [TN] ENIG solder joint embrittlement

        Per-Erik,

        Let me start off by saying I hate the name "Black Pad" because it
describes what a failure might look like but doesn't describe the type of
failure or root cause.  The historical Izod impact evaluations that were
done on solder joints  showed that a solder joint impact strength decreased
by approximately 50% when the gold concentration was between 3 and 5%.
Conservative reliability people usually use 3% as the gold embrittlement
value and those who have to get product out the door have a tendency to say
the value is 5%.  With the introduction of fine pitch SM parts and BGAs the
use of ENIG increased rapidly,  so did the brittle fractures which got the
name "Black Pad".  Since the ENIG defect rate was low and random those
investigating its cause tried to accelerate the defect level so that it
could be evaluated.  Unfortunately, when they began to use isothermal aging
it appears as if they introduced another failure mode.  Although the
defects
looked similar to "Black Pad" they were occurring with ENIG solder joints
that had as little as 0.3 wt.% gold.  When you do cross sectioning of
isothermal aged solder joints made to ENIG you see intermetallic layers at
the metallurgical interface to the copper.  I've seen cross sections that
sometime show what might be a AuNiSn IMC and at other times might be two
layers AuSn and NiSn IMCs.  I'm not a metallurgist and is some ways don't
care what the IMCs are but I do care that they form and weaken the
integrity/reliability of solder joints.  I've given up waiting for a "Black
Pad-Free" ENIG.  We use ENIG on some boards where it makes sense but for
the
majority of our boards we use immersion silver


        Regards,
        George

        George M. Wenger (908)-546-4531
        Reliability Engineer
        RF Power Amplifier Group
        Andrew Corporation,  40 Technology Drive, Warren, NJ 07059
        [log in to unmask]

                -----Original Message-----
                From: Tegehall Per-Erik [mailto:[log in to unmask]]
                Sent: Tuesday, October 14, 2003 3:24 AM
                To: [log in to unmask]
                Subject: Re: [TN] ENIG solder joint embrittlement


                George!

                I did not refer to the traditional form of gold
embrittlement. There are numerous papers showing that gold may cause a new
form of embrittlement when soldering to nickel surfaces. After soldering
the
gold will be find as AuSn intermetallic compounds evenly dispersed in the
solder joint. However, after some time, that is no longer the case. Most of
the gold will be found in a layer of AuNiSn IMC that is formed on top of
the
NiSn IMC layer on the nickel surface, which cause an embrittlement of the
solder joint. The higher the temperature, the faster this will happen. At
150 degree C, you may have an ebrittlement of the solder joint after 24
hours and it might happen if the gold concentration is higher than 0.3 %
and
it is likely that you get that if you have a plating with electrolytic
nickel/electrolytic gold on the component solder lands.

                For more information, se the following references:
                A. Eslambolchi, P. Johnson, M. Kaufmann och Z. Mei,
Electroless Ni/Immersion Au Evaluation - Final Program Report, Electronic
Assembly Development Center, Hewlett-Packard, Palo Alto, 1998.

                K. Zeng och K.N. Tu, Six Cases of Reliability Study of
Pb-free Solder Joints in Electronic Packaging Technology, Materials Science
and Engineering R, Vol. 38, 2002, sida 55-105.

                A. Zribi, R.R. Chromik, R. Presthus, K. Teed, L. Zavalij,
J.
DeVita, J. Tova, E.J. Cotts, J.A. Clum, R. Erich, A. Primavera, G. Westby,
R.J. Coyle och G.M. Wenger, Solder Metallization Interdiffusion in
Microelectronic Interconnects, IEEE Trans. on Comp. and Pack. Techn. Vol.
23, Nr. 2, 2000, sida 383-387.

                R. Darveaux, K. Banerji, A. Mawer och G. Dody, Reliability
of Plastic Ball Grid Array Assembly, J.H. Lau (Ed.), Ball Grid Array
Technology, McGraw-Hill, Inc., 1995, Kapitel 13.

                A.M Minor och J.W. Morris, Jr., Growth of Au-Ni-Sn
Intermetallic Compound on the Solder-Substrate Interface After Aging,
Metall. Mater. Trans, A, 31A, 2000, p. 789.
http://www.lbl.gov/morris/private/papers.html
<http://www.lbl.gov/morris/private/papers.html>

                A.M. Minor och J.W. Morris, Inhibiting Growth of the
Au0.5Ni0.5Sn4 Intermetallic Layer in Pb-Sn Solder Joints Reflowed on Au/Ni
Metallization, Journal of Electronic Materials, October 2000, Vol. 29,
Issue
10, sida 1170-1174. http://www.lbl.gov/morris/private/papers.html
<http://www.lbl.gov/morris/private/papers.html>


                Per-Erik Tegehall
                IVF, Sweden

                        -----Ursprungligt meddelande-----
                        Från: George Milad [mailto:[log in to unmask]]
                        Skickat: den 14 oktober 2003 04:45
                        Till: [log in to unmask]
                        Ämne: Re: [TN] ENIG solder joint embrittlement


                        The firgure reported by Glazer from Hp for gold
embrittlement was 3% and not 0.3%. The total amount of gold in ENIG if the
new IPC 4552 specification is followed is less than 5 micro-inches or 0.12
microns.
                        If one does the math, then it is evident that under
these conditions "Solder Joint Gold  Embrittlement" is a non issue for
ENIG.
                        Of course this is all on the board side and not the
component. If there is an issue with component side separation, the target
investigation should not be on ENIG leaving the true cause unidentified or
addressed.
                        Blaming the ENIG finish idiscrimanetly, and using
the "black Pad" as a catch all leaves a lot of areas, where things could go
wrong, unidentified and more important not corrected.
                        Blaming the "Black pad" is prevalent. I often
wonder
how prevalent the ture cases of "Black Pad" are?

                        George Milad
                        Uyemura International Corp
                        Chairman IPC Plating Commitee
                        ---------------------------------------------------
                        Technet Mail List provided as a free service by IPC
using LISTSERV 1.8e
                        To unsubscribe, send a message to [log in to unmask]
with following text in the BODY (NOT the subject field): SIGNOFF Technet
                        To temporarily halt or (re-start) delivery of
Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
                        To receive ONE mailing per day of all the posts:
send e-mail to [log in to unmask]: SET Technet Digest
                        Search the archives of previous posts at:
http://listserv.ipc.org/archives
                        Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information,
or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315

-----------------------------------------------------


                ---------------------------------------------------
                Technet Mail List provided as a free service by IPC using
LISTSERV 1.8e
                To unsubscribe, send a message to [log in to unmask] with
following text in the BODY (NOT the subject field): SIGNOFF Technet
                To temporarily halt or (re-start) delivery of Technet send
e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
                To receive ONE mailing per day of all the posts: send
e-mail
to [log in to unmask]: SET Technet Digest
                Search the archives of previous posts at:
http://listserv.ipc.org/archives
                Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information,
or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
                -----------------------------------------------------




----------------------------------------------------------------------------

--------------------
        This message is for the designated recipient only and may
        contain privileged, proprietary, or otherwise private information.
        If you have received it in error, please notify the sender
        immediately and delete the original. Any unauthorized use of
        this email is prohibited.

----------------------------------------------------------------------------

--------------------
        [mf2]
        ---------------------------------------------------
        Technet Mail List provided as a free service by IPC using LISTSERV
1.8e
        To unsubscribe, send a message to [log in to unmask] with following
text in the BODY (NOT the subject field): SIGNOFF Technet
        To temporarily halt or (re-start) delivery of Technet send e-mail
to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
        To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
        Search the archives of previous posts at:
http://listserv.ipc.org/archives
        Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information,
or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
        -----------------------------------------------------


---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
-----------------------------------------------------




---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------

ATOM RSS1 RSS2