<<1 anyway,
Again thanx.
It's pleasing to be able to dimension your little bits of knowledge, helps
join them up into something useful.
Regards
Mike
-----Original Message-----
From: Wenger, George M. [mailto:[log in to unmask]]
Sent: Friday, August 01, 2003 2:07 PM
To: [log in to unmask]; TechNet E-Mail Forum.
Subject: RE: [TN] Thick Palladium on Leads
Mike,
No and Yes.
No it isn't my data. Yes Wally has data for Ni. He only list data for
700F, 800F, and 900F
Tempeerature Radial dissolution rate 10-6in./sec.
at 700F 1.7
at 800F 4.4
at 900F 11.3
He also gives:
r = Ae(-B/T) where r is rate of dissolution in in./se. T is temperature in
degrees Rankine
Coefficient A for Ni =0.6
Cofficient B for Ni = 14,900
I know people have attempted to use the rate equaiton to find out what the
rate is at 450F but I tbink is is dangerous because Wally's rates were
established using a single thermally activated process and his work suggests
that there is more than one process contributing to the overall rate (e.g.,
diffusion in the metal, diffusion through the intermetallic compound layer,
transport in the liquid phase, etc.)
Regards,
George
George M. Wenger (908)-546-4531
Reliability Engineer
RF Power Amplifier Group
Andrew Corporation, 40 Technology Drive, Warren, NJ 07059
[log in to unmask]
-----Original Message-----
From: Mike Fenner [mailto:[log in to unmask]]
Sent: Friday, August 01, 2003 8:40 AM
To: TechNet E-Mail Forum.; Wenger, George M.
Subject: RE: [TN] Thick Palladium on Leads
This is an interesting thread.
Does your data give a number for Nickel?
Regards
Mike Fenner
Applications Engineer, European Operations
Indium Corporation
T: + 44 1908 580 400
M: + 44 7810 526 317
F: + 44 1908 580 411
E: [log in to unmask]
W: www.indium.com
Pb-free: www.Pb-Free.com
-----Original Message-----
From: TechNet [mailto:[log in to unmask]]On Behalf Of Wenger,
George M.
Sent: Thursday, July 31, 2003 6:54 PM
To: [log in to unmask]
Subject: Re: [TN] Thick Palladium on Leads
Bev,
How thick do you consider "thick undercoat"?
The NCMS PWB Surface Finishes work from several years ago looked at Pd
surface finishes. One issue with Pd is that it dissolves much slower than
other finishes. The best data I've seen on dissolution rates is the 1969
Wally Bader work published in the December Welding Journal.
For near eutectic SnPb solder at 450F
Material Radial Dissolution Rate (10-6in/sec)
Gold 117.9
Silver 43.6
Copper 4.1
Palladium 1.4
Regards,
George
George M. Wenger (908)-546-4531
Reliability Engineer
RF Power Amplifier Group
Andrew Corporation, 40 Technology Drive, Warren, NJ 07059
[log in to unmask]
-----Original Message-----
From: Bev Christian [mailto:[log in to unmask]]
Sent: Thursday, July 31, 2003 1:28 PM
To: [log in to unmask]
Subject: [TN] Thick Palladium on Leads
Technetters,
I have searched the archives and all I have been able to find is one
informative e-mail from Phil Hinton from August 22, 1998. Has anyone every
run across palladium as a thick undercoat? if so, what, if any, grief did
it cost you?
regards,
Bev Christian
Research in Motion
---------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
ext.5315
-----------------------------------------------------
----------------------------------------------------------------------------
--------------------
This message is for the designated recipient only and may
contain privileged, proprietary, or otherwise private information.
If you have received it in error, please notify the sender
immediately and delete the original. Any unauthorized use of
this email is prohibited.
----------------------------------------------------------------------------
--------------------
[mf2]
---------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
ext.5315
-----------------------------------------------------
::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::
:::
This email, its content and any files transmitted with it are intended
solely for the addressee(s) and may be legally privileged and/or
confidential. If you are not the intended recipient please delete and
contact the sender by return and delete the material from any computer. Any
review, retransmission, dissemination or other use of, or taking of any
action in reliance upon, this information by persons or entities other than
the intended recipient is prohibited.
Messages sent via this medium may be subject to delays, non-delivery and
unauthorized alteration. This email has been prepared using information
believed by the author to be reliable and accurate, but Indium Corporation
makes no warranty as to accuracy or completeness. In particular, Indium
Corporation does not accept responsibility for changes made to this email
after it was sent. Any opinions or recommendations expressed herein are
solely those of the author. They may be subject to change without notice.
::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::
:::
----------------------------------------------------------------------------
--------------------
This message is for the designated recipient only and may
contain privileged, proprietary, or otherwise private information.
If you have received it in error, please notify the sender
immediately and delete the original. Any unauthorized use of
this email is prohibited.
----------------------------------------------------------------------------
--------------------
[mf2]
:::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::
This email, its content and any files transmitted with it are intended solely for the addressee(s) and may be legally privileged and/or confidential. If you are not the intended recipient please delete and contact the sender by return and delete the material from any computer. Any review, retransmission, dissemination or other use of, or taking of any action in reliance upon, this information by persons or entities other than the intended recipient is prohibited.
Messages sent via this medium may be subject to delays, non-delivery and unauthorized alteration. This email has been prepared using information believed by the author to be reliable and accurate, but Indium Corporation makes no warranty as to accuracy or completeness. In particular, Indium Corporation does not accept responsibility for changes made to this email after it was sent. Any opinions or recommendations expressed herein are solely those of the author. They may be subject to change without notice.
:::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::
---------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------
|