Hi David! Collins conducted a series of gold wedge and gold ball bonding
test on immersion silver surface finishes and had only partial success. As
the immersion silver surface "aged" with storage time (3-6 months) we were
not able to create acceptable wirebonds. The initial bondability of the
finish in the as received condition was very good. There are a number of
folks who are successfully aluminum wiring bonding to the immersion silver
finish. Good luck.
Dave Hillman
Rockwell Collins
[log in to unmask]
davidyeh
<davidyeh@SINGNET To: [log in to unmask]
.COM.SG> cc:
Sent by: TechNet Subject: [TN] Gold wire bond on silver finishings
<TechNet@listserv
.ipc.org>
07/30/2003 09:21
PM
Please respond to
"TechNet E-Mail
Forum."; Please
respond to
davidyeh
Hi,
Can anyone share his experience on gold ball bonding on COB with immersion
silver finishings. What sort of silver thickness to ensure a good bonding
strength of min 3.5 gf?
We are using a 1 mil thick gold wire on a 6 to 20 microinch silver
thickness and encountered difficulty in achieving the min bonding strength
in wire pull.
Thanks for all inputs.
Best regards,
David.
---------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
ext.5315
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------
|
|
|