TECHNET Archives

August 2003

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
"TechNet E-Mail Forum." <[log in to unmask]>, Tony Steinke <[log in to unmask]>
Date:
Wed, 27 Aug 2003 19:51:33 +0200
MIME-version:
1.0
Reply-To:
"TechNet E-Mail Forum." <[log in to unmask]>, Gaby <[log in to unmask]>
Content-type:
text/plain; charset=iso-8859-1
Subject:
From:
Content-transfer-encoding:
7BIT
Parts/Attachments:
text/plain (190 lines)
Agree, but the solder mask adhesion to gold is not as good as on copper.
We had problems with solder mask adhesion during rework, and loosing solder
mask around pads on a large ground area or beteen the pad and the via is not
much fun when replacing BGA's.

Gaby


----- Original Message -----
From: "Tony Steinke" <[log in to unmask]>
To: <[log in to unmask]>
Sent: Wednesday, August 27, 2003 3:45 PM
Subject: Re: [TN] ENIG--Black Pad


> Werner, Bev,
>
> The soldermask process prior to ENIG plate is very critical(poor vacuum
> during exposing, developing, improper cure, poor oven ventilation,
> soldermask design, etc) and with my experience is probably a major cause
of
> the black pad syndrome. We process all ENIG boards as SMOG (soldermask
over
> gold). This eliminates alot of potential problems(yes, some may argue it
is
> a band-aid), but we have not experienced 1 panel with the black pad
> syndrome. The cost is a bit higher but it certainly out weighs a
> dissatisified customer(especially when you are building high end boards).
>
> Tony Steinke
> AIT-Atlanta Inc.
> ----- Original Message -----
> From: "Bev Christian" <[log in to unmask]>
> To: <[log in to unmask]>
> Sent: Wednesday, August 27, 2003 8:44 AM
> Subject: Re: [TN] ENIG--Black Pad
>
>
> Werner,
> Another theory I have heard espoused for black pad is that it occurs when
> there is preferential leaching of nickel into the gold plating bath from
> small pads electrically connected via traces and vias (sorry, pun) to
larger
> pads.  The large pads plate out properly, and first, leaving the smaller
> ones in contact with the relatively corrosive gold plating chemicals.
This
> would explain why the process in localized and why the higher phosphorus
> concentration.  However, I have no clue as to what would cause the
potential
> difference between the big and small pads.  And if people are seeing black
> pad with low phosphorus, this theory cannot explain that.
>
> I agree a technique - non-destructive, quick and inexpensive (where is a
> fairy godmother when you need one?) is needed.  ENIG is a good surface
> finish, but getting bitten, even at the overall average occurrence in the
> ppm level is NOT FUN.  At a previous company we ended up having to scrap
> over 2000 completed circuit packs because of black pad.  My problem with
the
> invitation to participate is that it INITIALLY came from students and
there
> was no background given in the invitation.  Now it did come from Siggi's
> e-mail address, but I think we should have got an introduction by him of
the
> students, if they are really interested in getting people to participate.
> If he is on holiday, then it should have been held off until his return.
> Siggi, are you there?
> regards,
> Bev Christian
> Research in Motion
>
> -----Original Message-----
> From: Werner Engelmaier [mailto:[log in to unmask]]
> Sent: August 27, 2003 8:28 AM
> To: [log in to unmask]
> Subject: [TN] ENIG--Black Pad
>
>
> Hi TechNetters,
> I had hoped to get a response/discussion to my posting repeated below. I
> would like to get peoples experiences to see whether the fit into scenario
A
> or B.
> Repeat:
> Yes, a method to detect problematic ENIG prior to assembly would be very
> useful--my problem is, that I do not know what such a method would be
> looking for.
> From my experience [but no research other than what other people write],
> what
> may be happening is as follows [please correct me, if I got it wrong and
> compare to your experience]:
> 1. during the Ni plating, P is co-deposited,
> 2. the amount of P varies with the plating bath/chemistry,
> At this point there seems to be some divirging opinions--maybe two
different
> processes--I split them up into scenarios A and B.
> 3A. Ni with too little P is subject to more corrosion during
> Au-plating--thus
> "Low-Phos" EN is bad--sulfur being dragged into the EN bath by solder mask
> also is implicated.
> 4A. A "loosely structured" nickel layer enriched in phosphorous is formed
> under the Au layer; this is sometimes called black-line nickel (BLN).
> 5A. Reflow soldering fails to form a consistent Sn/Ni IMC layer and a good
> metallurgical bond.
> 6A. "Brittle" interfacial fractures occur when loads are applied.
> CONSEQUENCE: The whole PCB surface would have this condition [I have not
> seen
> this].
> or
> 3B. During reflow, the Ni is consumed by the formation of the Sn/Ni IMC
> layer
> leaving P behind--the higher the P-content in Ni, the more Ni
concentration
> at the interface between Ni and Sn/Ni IMC--thus "High-Phos" EN is bad.
> 4B. The more heat [temperature x time] is available for IMC formation, the
> higher the P concentration.
> 5B. Nickel phosphide is formed creating a "weak link" adhesion between the
> Ni
> and the Sn/Ni IMC, even though good wetting has occurred.
> 6B. "Brittle" interfacial fractures occur when loads are applied.
> CONSEQUENCE: The "Black Pad" condition is worse in high peak reflow
profile
> areas--thus it is seemingly "localised" on the PCB; and typically the
> soldering
> pad has a crater-like rim of fractured ductile solder--rather than the
> "brittle" interfacial failure, perhaps because the P-concentration is less
> at the
> pad/ENIG area periphery. [this is more consistent with my observations].
>
> In either case, I do not know what one would be looking for on the
> as-received PWBs.
>
> Please give my--and the TechNet--youe feedback as to your observations; in
> particular, it would be interesting to get some Fab houses to respond with
> their
> experience.
>
> Werner Engelmaier
>
> ---------------------------------------------------
> Technet Mail List provided as a free service by IPC using LISTSERV 1.8e
> To unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt or (re-start) delivery of Technet send e-mail to
> [log in to unmask]: SET Technet NOMAIL or (MAIL)
> To receive ONE mailing per day of all the posts: send e-mail to
> [log in to unmask]: SET Technet Digest
> Search the archives of previous posts at: http://listserv.ipc.org/archives
> Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
> for additional information, or contact Keach Sasamori at [log in to unmask] or
> 847-509-9700 ext.5315
> -----------------------------------------------------
>
> ---------------------------------------------------
> Technet Mail List provided as a free service by IPC using LISTSERV 1.8e
> To unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt or (re-start) delivery of Technet send e-mail to
> [log in to unmask]: SET Technet NOMAIL or (MAIL)
> To receive ONE mailing per day of all the posts: send e-mail to
> [log in to unmask]: SET Technet Digest
> Search the archives of previous posts at: http://listserv.ipc.org/archives
> Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
> for additional information, or contact Keach Sasamori at [log in to unmask] or
> 847-509-9700 ext.5315
> -----------------------------------------------------
>
> ---------------------------------------------------
> Technet Mail List provided as a free service by IPC using LISTSERV 1.8e
> To unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
> To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
> Search the archives of previous posts at: http://listserv.ipc.org/archives
> Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
> -----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------

ATOM RSS1 RSS2