TECHNET Archives

August 2003

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
Werner Engelmaier <[log in to unmask]>, "TechNet E-Mail Forum." <[log in to unmask]>
Date:
Tue, 26 Aug 2003 12:58:09 +0530
Reply-To:
"TechNet E-Mail Forum." <[log in to unmask]>, anilkher <[log in to unmask]>
Subject:
MIME-Version:
1.0
Content-Transfer-Encoding:
7bit
Content-Type:
text/plain; charset="iso-8859-1"
From:
anilkher <[log in to unmask]>
Parts/Attachments:
text/plain (75 lines)
-----Original Message-----
From: anilkher [mailto:[log in to unmask]]
Sent: Tuesday, August 26, 2003 12:51 PM
To: 'Werner Engelmaier'; TechNet E-Mail Forum.
Subject: RE: Black Pad Detecting Machine


Rather than AOI could we not use a random scan EDX for P/NI ratio under
Gold layer?? Anil Kher

-----Original Message-----
From: Werner Engelmaier [mailto:[log in to unmask]]
Sent: Monday, August 25, 2003 10:38 PM
Subject: Re: Black Pad Detecting Machine


Hallo Elisabeth and Christian,
Yes, a method to detect problematic ENIG prior to assembly would be very
useful--my problem is, that I do not know what such a method would be
looking for. From my experience [but no research other than what other
people write], what is happening is as follows [please correct me, if I
got it wrong]: 1. during the Ni plating, P is co-deposited, 2. the
amount of P varies with the plating bath/chemistry, At this point there
seems to be some divirging opinions--maybe two different processes--I
split them up into paths A and B. 3A. Ni with too little P is subject to
more corrosion during Au-plating--thus "Low-Phos" ENi is bad--sulfur
dragged into the EN bath by solder mask also is implicated. 4A. A
"loosely structured" nickel layer enriched in phosphorous is formed
under the Au layer; this is sometimes called black-line nickel (BLN).
5A. Reflow soldering fails to form a consistent Sn/Ni IMC layer and a
good metallurgical bond. 6A. "Brittle" interfacial fractures occur when
loads are applied.
CONSEQUENCE: The whole PCB surface would have this condition. or 3B.
During reflow, the Ni is consumed by the formation of the Sn/Ni IMC
layer leaving P behind--the higher the P-content in Ni, the more Ni
concentration at the interface between Ni and Sn/Ni IMC--thus
"High-Phos" EN is bad. 4B. The more heat [temperature x time] is
available for IMC formation, the higher the P concentration. 5B. Nickel
phosphide is formed creating a "weak link" adhesion between the Ni and
the Sn/Ni IMC, even though good wetting has occurred. 6B. "Brittle"
interfacial fractures occur when loads are applied.
CONSEQUENCE: The "Black Pad" condition is worse in high peak reflow
profile areas--thus it is seemingly "localised" on the PCB; and
typically the soldering pad has a crater-like rim of fractured ductile
solder--rather than the "brittle" interfacial failure, perhaps because
the P-concentration is less at the pad/ENIG area periphery.

In either case, I do not know what one would be looking for on the
as-received PWBs.

Werner Engelmaier

---------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text
in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt
or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
archives of previous posts at: http://listserv.ipc.org/archives Please
visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------

ATOM RSS1 RSS2