Hi guys and the answer is yes each pass through a solder temp cycle
destoyes the board a little more. most .062 1 oz plated boards can only
withstand 2 or 3 cycles before they start to crack at the via to joint. now
as most things are cumilitive and definable it may take 4-5 to acualy open
but I have and can easly find cracks starting as low as 2 cycles. remeber
the board manufacturer takes two cycles away because he hot oil reflows and
he oven cures for solder mask. I have a chart where I did a test of copper
thickness vers's heat cycles. 1 oz fialed in 5 to 7 cycles ( no pcb
manufatures cycles) 2 oz survived 7 to 12 3 oz 15 to 20 4 oz threough 10 oz
were not realy affected. it appears that the heaver copper vias are able to
resist the push of the expansion forces happening when you solder. the
initial question was does high temp affect a board and the answer is more
then you think. So if you want a very reliable board add extra plating, this
can be done quite easly by starting with 1/4 oz copper and use 3 or 4 mil
dry film and plate up . The etching is faster and the line definition will
be much better, but best of all your board will withstand twice the relfow
solder cycles.
Robert tarzwell author of high powered printed circuits and, flex
circuit design Megadawn.com
---------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------
|
|
|