Hi Rob,
The IPC server strips attachments--you could try imbedding a photo into the
main message or send it directly to me.
If your problem occurs after HASL, a couple of possibilities exist [ordered
in sequence of decreasing likelihood]--all of these possibilities point to a
very high z-expansion of the resin.
1. the prepreg layers are undercured and expand to much;
2. your HASL temperature is too high;
3. your material is not FR-4 glass-reinforced, but reinforced with something
like Kevlar.
Werner Engelmaier
Engelmaier Associates, L.C.
Electronic Packaging, Interconnection and Reliability Consulting
7 Jasmine Run
Ormond Beach, FL 32174 USA
Phone: 386-437-8747, Fax: 386-437-8737, Cell: 386-316-5904
E-mail: [log in to unmask], Website: www.engelmaier.com
---------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------
|
|
|