Hi Bill,
here are a few references (paraphrased). There's additional info in the
sections.
IPC-4101 section 3.8.3.1.6
h. voids are <0.075mm [0.0029"] in the longest dimension & don't occur in
void clusters any more than 3 voids in a 3.2mm circle.
IPC-A-600 section 3.1.1
Acceptable- Class 2 & 3
Voids less than or equal to 0.08mm [0.0031"] and doesn't violate minimum
dielectric spacing.
IPC-6012A section 3.6.2.3
No laminate voids in excess of 0.00315" (in Zone B).
Regards,
Mark
-----Original Message-----
From: Brown, William G [SMTP:[log in to unmask]]
Sent: Tuesday, April 22, 2003 1:45 PM
To: [log in to unmask]
Subject: [TN] Voids / Air Pockets in Laminates
Hi All,
Does anyone know where I can find information on air bubbles or
voids within
completed circuit boards? We have a group here which is concerned
about any
voids left when the laminates are pressed together, either within or
between
layers, and the effects they might have at high altitudes.
Are there any IPC specs which state allowable values or anything
like that?
These are boards made with IPC-4101/ 40, 41 or 42 materials.
Thanks for any help!
Bill
############################################
William G. Brown
Senior Electrical Engineer - PWD Engineering Support
> xBAE SYSTEMSx - Information & Electronic Warfare Systems
Phone: 603-885-4930 Fax: 603-885-5435
############################################
---------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV
1.8e
To unsubscribe, send a message to [log in to unmask] with following
text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for
additional
information, or contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------
|
|
|